A method for preparing electrolytic cathode material by doping metal and nitrogen with phenolic resin and its application

By using phenolic resin or waste phenolic resin doped with nitrogen and metal salts, nitrogen doped with metal salts, the problem of low BPA removal efficiency in traditional water treatment technology is solved, and efficient BPA contaminated water treatment is achieved and Reuse of waste materials.

CN115872498BActive Publication Date: 2024-11-15TONGJI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211525645.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-01
Publication Date
2024-11-15
Estimated Expiration
2042-12-01

AI Technical Summary

Technical Problem

Traditional water treatment technology has low efficiency in removing bisphenol A, and electrolytic technology is difficult to effectively degrade BPA contaminated water. The existing electrode materials have poor effect on BPA treatment.

Method used

Phenolic resin or waste phenolic resin is used as carbon-based materials, doped with nitrogen and metal salts, and nitrogen doped with metallic salts to prepare nitrogen-doped metal carbon cathode plate materials, and the removal rate of BPA is increased through the electrolysis process.

Benefits of technology

The degradation rate of BPA pollutants is significantly improved, the recycling of waste phenolic resin is realized, the treatment cost is reduced, and the efficient removal effect is maintained within the pH value and current density range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115872498B_ABST
    Figure CN115872498B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of polluted water treatment, and relates to a method for preparing an electrolytic cathode coating material. The method includes: obtaining a metal salt solution, a nitrogen component precursor, and a phenolic resin powder; the metal salt solution is a salt solution mixture of any one or more of transition metal iron, cobalt, and nickel; the nitrogen component precursor is selected from one or more of urea, aniline, and dicyandiamide; the phenolic resin powder is formed by crushing waste phenolic resin into powder; the metal salt mass is 0.05-3.0wt% of the resin mass; the above mixture is mixed under high temperature conditions to form a powder, and polyvinylidene fluoride and carbon black are added, and the powder is obtained after grinding and ultrasonic treatment. The raw material source of the present invention is easy to obtain and cheap, the preparation process is simple, the cost is low, and the efficiency is high, and the waste phenolic resin and bisphenol A polluted water can be treated at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polluted water treatment, and specifically relates to the use of phenolic resin or waste phenolic resin as a carbon-based material to prepare a nitrogen-doped metal carbon cathode plate material for electrolyzing bisphenol A wastewater. Background Art

[0002] Bisphenol A (BPA) is an important organic chemical raw material, mainly used in the production of polymer materials such as polycarbonate, epoxy resin, polysulfone resin, polyphenylene ether resin, unsaturated polyester resin, etc. It can also be used in the production of fine chemicals such as coatings, antioxidants, plasticizers, flame retardants, rubber aging agents, and heat stabilizers. In the production process of plastic products, the addition of BPA can make plastics colorless, transparent, durable, lightweight, and impact-resistant, and has the characteristics of preventing acidic substances from corroding metals. Therefore, BPA is widely used in the production process of hundreds of daily necessities such as food packaging, beverage bottles, milk bottles, and glasses. With the use of BPA, it is found that BPA can penetrate from products into food and water, causing negative impacts on the environment and human health. Studies have shown that BPA in the environment, as an endocrine disruptor, enters the environmental medium through discharge, accumulates in animals and humans through the amplification of the food chain, and may produce greater toxic effects. At the same time, BPA has been widely detected in natural water environments and engineering water systems. Such substances diffuse in aquatic ecosystems and have high environmental risks. This poses a challenge to the field of water management, and the problem of treating contaminated water containing BPA needs to be solved urgently.

[0003] Research data shows that the BPA removal rate of traditional water treatment technology after coagulation, sedimentation and sand filtration is only about 25%, indicating that conventional processes and activated carbon adsorption have very limited BPA removal efficiency. Electrolytic treatment of wastewater is based on the principle of electrolysis, which causes pollutants in wastewater to undergo reduction and oxidation reactions at the cathode or anode through the electrolysis process to achieve wastewater purification. Electrolysis technology is effective in improving the removal of difficult-to-degrade pollutants such as BPA that are difficult to remove by conventional means. Summary of the invention

[0004] The technical problem to be solved by the present invention is to comprehensively consider the BPA water pollution and the advantages of electrolysis technology, and provide a new electrode plate material that can be used for enhanced electrolysis purification of BPA wastewater.

[0005] In the first aspect, the present invention provides a method for preparing an electrolytic cathode coating material, the method comprising the following steps: obtaining a metal salt solution, a nitrogen component precursor, and a phenolic resin powder; the metal is one or more of transition metals such as iron, cobalt, and nickel. The mass of the metal salt is 0.05-3.0wt% of the mass of the resin, and the mass ratio of the nitrogen component precursor to the metal salt plus the mass of the phenolic resin powder is 5%-10%, and the mass ratio is measured by mass ratio; the above mixture is cured and pyrolyzed, and then ground into powder, and polyvinylidene fluoride and carbon black are added, and the mixture is ground and ultrasonically treated to obtain the obtained mixture.

[0006] In the present invention, nitrogen doping is to add a certain amount of nitrogen component precursor, such as urea, aniline, dicyandiamide, etc., to the raw material. The nitrogen component precursor of the present invention is selected from one or more of urea, aniline, and dicyandiamide.

[0007] Preferably, the metal salt solution is a mixture of salt solutions of any one or more of transition metals iron, cobalt, and nickel; the metal salt can be selected from one or more of (Fe(NO3)3, Co(NO3)2, Ni(NO3)2.

[0008] The phenolic resin powder is a powder containing phenolic resin. Preferably, the phenolic resin is crushed to form a powder; various phenolic resins can be used, especially waste phenolic resins. The present invention transforms waste phenolic resins so that they can be doped with metal salts and prepared into electrode coating materials with the ability to eliminate bisphenol A.

[0009] Preferably, the above preparation process specifically includes the following steps:

[0010] (1) mixing phenolic resin powder and metal salt solution uniformly, and drying and solidifying the mixture;

[0011] (2) adding a nitrogen component precursor to the dried and solidified mixture and mixing them evenly;

[0012] (3) pyrolyzing a mixture containing a phenolic resin, a metal salt and a nitrogen component precursor at a constant temperature of 700-1000° C. for 3-5 hours under an inert gas atmosphere, and cooling naturally to obtain a solid product;

[0013] (4) grinding into powder, washing with ethanol and deionized water alternately, and vacuum drying to obtain nitrogen-doped metal composite carbon material;

[0014] (5) adding polyvinylidene fluoride and carbon black to the nitrogen-doped metal composite carbon material and grinding them evenly;

[0015] (6) Add methyl pyrrolidone and perform ultrasonic treatment to prepare nitrogen-doped metal carbon slurry.

[0016] Preferably, in the above preparation process, the pyrolysis time can be shortened, for example, 2-4 hours. The pyrolysis temperature can also be controlled within a smaller range, for example, 800-900° C., so as to obtain a better preparation effect.

[0017] In a preferred embodiment of the present invention, phenolic resin powder and metal salt solution are mixed evenly, and the mixture is dried and solidified; urea is used as a nitrogen component precursor, urea solid is added to the solidified body of metal salt and phenolic resin, and the mixture is mixed evenly, and the mass ratio of urea to solidified material is controlled to be 5%-10%; pyrolysis is carried out at a constant temperature of 700-1000°C for 3-5h under an inert gas atmosphere; the black solid product is naturally cooled to room temperature to obtain a black solid product, ground into powder, and washed alternately with ethanol and deionized water for several times, and vacuum dried for standby use; 3-5mg of nitrogen-doped metal composite carbon material is weighed, 5.0mg of polyvinylidene fluoride and 5.0mg of carbon black are added, poured into a quartz mortar, ground evenly, transferred to a centrifuge tube, 0.9mL of methyl pyrrolidone is added for ultrasonication, and nitrogen-doped metal carbon slurry is prepared for standby use.

[0018] In a second aspect, the present invention provides an electrolytic cathode coating material, wherein the electrolytic cathode coating material comprises a metal salt solution, a nitrogen component precursor, and a phenolic resin powder. Preferably, the electrolytic cathode coating material is obtained using the above-mentioned preparation method of the electrolytic cathode coating material.

[0019] In a third aspect, the present invention provides an electrolytic cathode, which is obtained by coating the above-mentioned electrolytic cathode coating material on the surface of an electrode plate.

[0020] Preferably, the coating process can be: take an appropriate amount of nitrogen-doped metal carbon slurry and evenly apply it to the front and back of the titanium sheet, apply it once every period of time until the titanium sheet is evenly coated. Dry the titanium sheet loaded with the slurry until the water is removed and it does not crack, and the obtained material is the nitrogen-doped metal carbon cathode plate material.

[0021] Preferably, the nitrogen-doped metal carbon slurry used generally depends on the electrode plate area, volume and usage scenario. For example, in a laboratory, no less than 2 μL of nitrogen-doped metal carbon slurry, such as 3-50 μL, 5-20 μL, etc., can be used for electrode coating.

[0022] In a fourth aspect, the present invention provides an application of the electrolytic cathode coating material or a preparation method thereof. Based on the problem of BPA-contaminated wastewater in the field of water treatment in the environment, the present invention uses phenolic resin or waste phenolic resin as a carbon-based material, doped with nitrogen and metal salts mixed into carbon-making raw materials, prepares nitrogen-doped metal carbon materials, and coats them on the electrode plates of the electrolytic cell as cathodes, thereby improving the electrolysis efficiency and strengthening the treatment of BPA wastewater.

[0023] Preferably, the electrolytic cathode coating material is coated on the surface of the electrode plate to form an electrolytic cell cathode plate for degrading bisphenol A in the liquid. The phenolic resin used can be an industrial phenolic resin raw material or a collected waste product with phenolic resin as the main raw material. In view of the current situation that waste phenolic resin is effectively treated and bisphenol A contaminated water is widely present, the present invention simultaneously realizes the treatment of waste phenolic resin and bisphenol A wastewater, so that the two pollution problems are effectively solved at the same time.

[0024] Preferably, the process of degrading bisphenol A comprises the following steps:

[0025] S1, coating the electrolytic cathode coating material on the surface of the electrode plate to form an electrolytic cell cathode plate;

[0026] S2, installing the cathode plate and anode plate of the electrolytic cell in the electrolytic cell, and using a conventional oxidation electrode as the anode;

[0027] S3, placing the liquid from which bisphenol A is to be removed in an electrolytic cell;

[0028] S4, during the electrolysis process, the pH value of the liquid ranges from 0 to 11, and the concentration of bisphenol A is not greater than 30 mg / L.

[0029] Preferably, the pH value range of the liquid to be removed of bisphenol A is not greater than 11, such as 1-10, 3-9, or pH=4, pH=5, pH=6, etc. In practice, the pH value range can be determined by taking into account the cost and equipment facilities of sewage treatment.

[0030] Preferably, the concentration of bisphenol A ranges from 1 to 20 mg / L, such as 2 to 20, 3, 5, 8, 10, 12, 15 mg / L, etc. When testing the effect in the laboratory, the bisphenol A wastewater can use a bisphenol A aqueous solution of a certain concentration prepared using bisphenol A material of standard purity.

[0031] Preferably, the current density may be a lower current intensity not greater than 50 mA, such as 10, 20, 30, 40, 50 mA, etc.

[0032] The electrolyte can use a conventional electrolyte. In a preferred embodiment of the present invention, the current density is 40 mA, the electrode spacing is 0.5 cm, the electrolyte Na2SO4 concentration is 5 mM, the pH value is 7.0, and the electrolysis time is 1 hour. Oxygen can also be introduced during the electrolysis process to further improve the efficiency of the electrolysis.

[0033] The present invention is based on the practical possibility of electrolysis technology in removing BPA pollution in water bodies. By modifying carbon materials by nitrogen doping and loading metals, an electrode material for efficiently degrading BPA wastewater based on electrolysis is provided. Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. The prepared nitrogen-doped metal carbon cathode plate material has a high degradation rate of BPA pollutants in electrolysis, has great advantages in treating BPA wastewater, and is also expected to be used in the treatment of other organic wastewater.

[0035] 2. It realizes the recycling of waste phenolic resin, which is in line with the dual carbon concept.

[0036] 3. The raw materials for the preparation of the present invention are easily available and inexpensive, the preparation process is simple, and less equipment is required. It has obvious advantages such as less initial investment, low cost, and high efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the embodiments will be briefly introduced below. Obviously, each drawing in the following description is for some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0038] Figure 1 The microstructure of nitrogen-doped metal carbon cathode material.

[0039] The scale of Figure (a) is 1:10 μm, and the scale of Figure (b) is 1:1 μm.

[0040] Figure 2 The effect of adding different metals on the degradation of BPA.

[0041] Figure 3 The effect of pollutant concentration on electrolytic BPA wastewater.

[0042] Figure 4 The effect of current density on the electrolysis of BPA wastewater.

[0043] Figure 5 The effect of pH value on electrolysis of BPA wastewater.

[0044] Figure 6 Schematic diagram of the device for degrading BPA using nitrogen-doped cobalt metal cathode. DETAILED DESCRIPTION

[0045] The present invention relates to a material for preparing electrolytic cathode degradation of bisphenol A wastewater by doping phenolic resin with metal and nitrogen. A metal salt solution, a nitrogen-containing substance and waste phenolic resin powder are mixed in a certain proportion, and a nitrogen-doped metal carbon material can be prepared according to the preparation method, which is coated on an electrode substrate to prepare an electrolytic cell cathode plate, and is used for the electrolytic efficient treatment of bisphenol A wastewater.

[0046] Compared with the prior art, the present invention realizes the comprehensive utilization of waste phenolic resin and the degradation of bisphenol A wastewater by preparing an electrolytic cathode plate, and the removal effect of bisphenol A is significantly improved in the process of turning waste into treasure.

[0047] The technical solution will be clearly and completely described below through the embodiments of the present application. Obviously, the described embodiments are only part of the preferred embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present application.

[0048] Collect phenolic resin or waste phenolic resin ground into powder, dissolve a certain amount of metal salt in anhydrous ethanol, the metal salt can be one or more of (Fe(NO3)3, Co(NO3)2, Ni(NO3)2. Mix the phenolic resin powder and the metal salt solution evenly, control the metal mass to be 0.05-3.0wt% of the resin mass, and further dry the mixture for 12-36h to solidify. Add urea solid, mix the metal salt and the solidified body of phenolic resin evenly, and control the mass ratio of urea to solidified material to be 5%-10%. Pyrolyze at a constant temperature of 700-1000°C for 3-5h in an inert gas atmosphere. After completion, naturally cool to room temperature to obtain The black solid product is further ground into powder, washed alternately with ethanol and deionized water several times, and then vacuum dried for use. Weigh 3-5 mg of the prepared nitrogen-doped metal composite carbon material, add 5.0 mg of polyvinylidene fluoride and 5.0 mg of carbon black, pour into a quartz mortar and grind evenly, transfer to a centrifuge tube, add 0.9 mL of methyl pyrrolidone and ultrasonicate to prepare nitrogen-doped metal carbon slurry for use. Transfer 5-20 μL of nitrogen-doped metal carbon slurry and apply it evenly to the front and back of the titanium sheet, and apply it once every once in a while until the titanium sheet is evenly coated. Dry the titanium sheet loaded with the slurry until the water is removed and it does not crack, and the resulting nitrogen-doped metal carbon cathode plate material is then used for the electrolytic cell degradation of BPA wastewater experiment.

[0049] The synthesized nitrogen-doped metal carbon cathode material was first characterized at room temperature. Figure 1 As shown, the nitrogen-doped metal carbon material was characterized by scanning electron microscopy. The surface of the nitrogen-doped metal carbon material was coral-like, and the rough surface increased the specific surface area of ​​the material, which was conducive to the adsorption of pollutants.

[0050] In the following examples, the electrolytic cell anode uses a common platinum electrode, and the cathode plate uses the prepared preferred nitrogen-doped cobalt metal carbon cathode plate material, and the effects of different conditions on the electrolytic degradation rate of BPA are studied respectively.

[0051] Example 1

[0052] The performance test of the electrode plates prepared under different metal doping was carried out. Three composite carbon materials of 1wt% Fe, 1wt% Ni, and 1wt% Co were prepared. The initial electrolysis conditions were set as follows: BPA initial concentration 5.0mg / L, current density 40mA, electrode spacing 0.5cm, electrolyte Na2SO4 concentration 5mM, pH 7.0, electrolysis time 1h, and the carbon material without nitrogen and metal doping was used as a blank experiment. Figure 2 As shown in the figure, the type of carbon cathode material significantly affects the effect of electrolytic degradation of BPA. The BPA degradation rates of carbon cathodes doped with different metals (nickel, iron, cobalt) reached 50.48%, 45.19%, and 75.67%. Compared with the blank group (33.77%) without nitrogen-doped metal carbon material, the electrolytic removal rate of BPA can be effectively improved, among which the nitrogen-doped cobalt metal carbon cathode showed excellent performance in degradation of organic pollutants.

[0053] Example 2

[0054] The effect of different pollutant concentrations on the electrolytic degradation of BPA was tested using a nitrogen-doped cobalt metal cathode. The initial electrolysis conditions were set as follows: BPA concentration (1.0, 2.0, 5.0, 10.0, 20.0 mg / L), current density 40 mA, electrode spacing 0.5 cm, electrolyte Na2SO4 concentration 5 mM, pH 7.0, and electrolysis time 1 h. Figure 3 As shown, the electrolytic BPA removal rates within 1 hour were 78.01%, 70.46%, 65.67%, 51.61% and 46.06%, respectively, and the BPA degradation rate decreased with the increase of pollutant concentration.

[0055] Example 3

[0056] The effect of different pollutant concentrations on the electrolytic degradation of BPA was tested using a nitrogen-doped cobalt metal cathode. The initial electrolysis conditions were set as follows: BPA initial concentration 5.0 mg / L, current density (10, 20, 30, 40, 50 mA), electrode spacing 0.5 cm, electrolyte Na2SO4 concentration 5 mM, pH 7.0, and electrolysis time 1 h. Figure 4 As shown, the electrolytic BPA removal rates within 1 hour were 47.42%, 57.14%, 61.28%, 65.67% and 68.46%, respectively, and the BPA degradation rate increased with the increase of current density; but with the increase of current density, the increase of degradation rate slowed down, indicating that the prepared cathode plate can also show good electrolytic pollution reduction performance at a lower current density.

[0057] Example 4

[0058] The effect of different pollutant concentrations on the electrolytic degradation of BPA was tested using a nitrogen-doped cobalt metal cathode. The initial electrolysis conditions were set as follows: BPA initial concentration 5.0 mg / L, current density 40 mA, electrode spacing 0.5 cm, electrolyte Na2SO4 concentration 5 mM, pH value (3.0, 5.0, 7.0, 9.0, 11.0), and electrolysis time 1 h. Figure 5 As shown in the figure, the electrolytic BPA removal rates within 1 hour were 65.67%, 73.64%, 74.8%, 88.14% and 70.12%, respectively. Under different pH environments, the BPA electrolysis rate was high and the water pH value increased first and then decreased, with the optimal pH value being around 9.0. The results showed that the prepared nitrogen-doped cobalt metal cathode plate had a wide pH application range, and the optimal pH working point did not require a large amount of acid-base regulators.

[0059] The above results show that the synthesized nitrogen-doped metal carbon cathode plate material electrolyzes BPA wastewater, and its electrolytic removal rate is higher than that of nitrogen-free and metal-doped carbon cathode plates, and the cathode plate has good electrolytic pollution reduction performance under various conditions, indicating that the nitrogen-doped metal carbon cathode plate material prepared by the present invention can be used as an electrolytic cathode plate to efficiently degrade BPA wastewater.

[0060] The above-described embodiments are only specific implementation methods of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be thought of by any technician familiar with the art within the technical scope disclosed in the present application without creative work should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims in the present application.

Claims

1. A method for preparing an electrolytic cathode coating material, characterized in that: The preparation method of the electrolytic cathode coating material comprises the following steps: Obtain a metal salt solution, a nitrogen component precursor, and a phenolic resin powder; the metal salt solution is a mixture of any one or more salt solutions of transition metals iron, cobalt, and nickel; the nitrogen component precursor is selected from one or more of urea, aniline, and dicyandiamide; the phenolic resin powder is formed by crushing waste phenolic resin; the mass of the metal salt is 0.05-3.0wt% of the mass of the resin, and the mass ratio of the nitrogen component precursor to the sum of the mass of the metal salt and the mass of the phenolic resin powder is 5%-10%, and the proportion is measured by mass ratio; The mixture is pyrolyzed into powder, and polyvinylidene fluoride and carbon black are added, and the powder is obtained after grinding and ultrasonic treatment.

2. The method for preparing the electrolytic cathode coating material according to claim 1, characterized in that: First, the phenolic resin powder and the metal salt solution are mixed evenly, and the mixture is dried and solidified; second, adding a nitrogen component precursor to the dried and solidified mixture and mixing them evenly; Third, in an inert gas atmosphere, a mixture containing phenolic resin, metal salt and nitrogen component precursor is pyrolyzed at 700-1000° C. for 3-5 hours, and naturally cooled to obtain a solid product; Fourth, grinding the solid product into powder, washing it alternately with ethanol and deionized water, and vacuum drying it to obtain a nitrogen-doped metal composite carbon material; Fifth, adding polyvinylidene fluoride and carbon black to the nitrogen-doped metal composite carbon material and grinding them evenly; Sixth, add methyl pyrrolidone and ultrasonically prepare nitrogen-doped metal carbon slurry.

3. The method for preparing the electrolytic cathode coating material according to claim 1, characterized in that: The phenolic resin powder and the metal salt solution are mixed evenly, and the mixture is dried and solidified; urea solid is added to the solidified body of the metal salt and the phenolic resin and mixed evenly, and the mass ratio of urea to the solidified material is controlled to be 5%-10%; the product is pyrolyzed at a constant temperature of 700-1000°C for 3-5h in an inert gas atmosphere; the product is naturally cooled to room temperature to obtain a black solid product, which is ground into powder in a mortar, and is alternately washed with ethanol and deionized water for several times and vacuum dried for use; 3-5mg of nitrogen-doped metal composite carbon material is weighed, 5.0mg of polyvinylidene fluoride and 5.0mg of carbon black are added, poured into a quartz mortar and ground evenly, and the product is transferred to a centrifuge tube, 0.9mL of methyl pyrrolidone is added and ultrasonicated to prepare a nitrogen-doped metal carbon slurry for use.

4. An electrolytic cathode coating material, characterized in that: The electrolytic cathode coating material is obtained using the preparation method of the electrolytic cathode coating material according to claim 1.

5. An electrolytic cathode, characterized in that: The electrode plate is obtained by coating the electrolytic cathode coating material according to claim 4 on the upper surface.

6. The use of the electrolytic cathode coating material according to claim 4, characterized in that: The electrolytic cathode coating material is coated on the surface of the electrode plate to form an electrolytic cell cathode plate, which is used to degrade bisphenol A in liquid and simultaneously treat waste phenolic resin and bisphenol A wastewater.

7. The use of the electrolytic cathode coating material according to claim 6, characterized in that: The process of degrading bisphenol A comprises the following steps: S1, coating the electrolytic cathode coating material on the surface of the electrode plate to form an electrolytic cell cathode plate; S2, installing the cathode plate and anode plate of the electrolytic cell in an electrolytic cell, and using an oxidation electrode as the anode; S3, placing the liquid from which bisphenol A is to be removed in an electrolytic cell; S4, during the electrolysis process, the pH value of the liquid to be removed of bisphenol A is in the range of 0-11, and the concentration of bisphenol A is not greater than 30 mg / L.