A green, environmentally friendly, energy-saving water-based ink printing process
Patent Information
- Application Number
- CN202211565651.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-07
AI Technical Summary
[0004]本发明旨在提供一种绿色环保型节能水性油墨印刷工艺,用解决现有水性油墨印刷技术在pH值上难以把控的技术问题
[0022] 1. The present invention adds an acid-beating step on the basis of existing printing. It relaxes the pH value control range of the water-based ink during the printing process, facilitates operation, improves the pH value of the water-based ink, and can also reduce the viscosity of the water-based ink and improve the printing process. Fluidity, which helps improve the smooth performance of inkjet;
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water-based ink printing, and in particular to a green, environment-friendly and energy-saving water-based ink printing process. Background Art
[0002] The ink used in traditional inkjet printing technology has a large content of organic solvents, and the VOCs pollution generated during the production process not only seriously harms the environment, but also has a great impact on the health of the staff. Based on this, the publication number CN113619306A provides a green environmentally friendly printing process, which effectively improves the viscosity of the ink and enhances its adhesion by adding titanium dioxide and sodium carboxymethyl cellulose to the ink raw materials. At the same time, the printing process is simple, environmentally friendly and energy-saving, and the printing cost is low. During the printing process, the printing is photographed in real time by a camera to obtain a printed image. By analyzing the printed image, it is determined whether the printing process meets the green environmental protection printing standard. If it does not meet the requirements, the printing parameters are adjusted in real time to ensure the green environmental protection of the entire printing process. However, this technology does not essentially reduce the organic solvents in the ink, and the VOCs pollution generated during the production process has not changed substantially. Secondly, the increase in ink viscosity will increase the drying speed, but the increase in viscosity will cause the fluidity of the ink to decrease, which will also cause defects such as dirty plates, paste plates, and bubbling.
[0003] With the advent of water-based inks, based on the low organic solvent characteristics of water-based inks, people have also found that if water-based inks are used instead of traditional inks, Vocs pollution can be greatly reduced. In the scheme with publication number CN113354982A, a printing technology that uses water-based inks instead of traditional inks is actually disclosed. However, during the printing process of water-based inks, the pH value needs to be strictly controlled. When the pH value is higher than 9.5, the alkalinity is too strong, the viscosity of the ink will decrease, the drying speed will slow down, and the water resistance will deteriorate; and when the pH value is lower than 8, the alkalinity is too weak, the viscosity of the ink will increase, the drying speed will accelerate, and it will cause defects such as dirty plates, paste plates, and bubbles. Therefore, this technology is difficult to control the pH value. Summary of the invention
[0004] The present invention aims to provide a green, environment-friendly and energy-saving water-based ink printing process, so as to solve the technical problem that the pH value of the existing water-based ink printing technology is difficult to control.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A green, environmentally friendly, energy-saving water-based ink printing process comprises the following steps:
[0007] (1) Cleaning the printing substrate A: Clean the surface of the printing substrate to make it dust-free and keep it clean, and then fix it to a designated position;
[0008] (2) Acid printing: Use dilute acid instead of ink to print first to obtain printing substrate B;
[0009] (3) Spraying water-based ink: After positioning again, a water-based ink with a pH value ranging from 8 to 11 is printed on the acidic printed matter of the printing substrate B to obtain a printed matter C;
[0010] (4) Drying and curing: In a confined space, the printed material C is dried and cured by an infrared drying device, and the confined space is evacuated and ventilated before the device is turned on;
[0011] (5) Cooling treatment: The dried and solidified product is transferred to a cooling room and cooled by refrigeration equipment. The printed product is obtained by cooling it to room temperature.
[0012] Preferably, the dilute acid solution in step (2) is dilute hydrochloric acid with a pH value of 3 to 5, and its usage amount is 20% to 30% of the water-based ink used for printing.
[0013] Preferably, the aqueous ink used in step (3) is a commercially available aqueous ink, and the pH value of the aqueous ink is controlled to be in the range of 8 to 11 using an acid-base buffer solution with a pH value in the range of 8 to 11 before use.
[0014] Furthermore, the acid-base buffer is one of glycine-sodium hydroxide buffer, borax-sodium hydroxide buffer, and sodium carbonate-sodium bicarbonate buffer.
[0015] Preferably, the specific ingredients of the aqueous ink used in step (3) are, by weight: 25 to 30 parts of pigment, 20 to 25 parts of water-soluble synthetic resin, 5 to 10 parts of glycerol, 5 to 10 parts of vegetable oil, 4 to 6 parts of fatty acid methyl ester, 2 to 3 parts of dispersant, 0.5 to 1 part of antioxidant, and 0.5 to 1 part of defoaming agent.
[0016] Furthermore, the vegetable oil is one or more of soybean oil, corn oil, sunflower oil, tung oil, and peanut oil.
[0017] Furthermore, the dispersant is a metal soap substance.
[0018] Furthermore, the antioxidant is one or more of tea polyphenols, tocopherol, flavonoids, butylated hydroxyanisole, butylated hydroxytoluene, and tert-butylhydroquinone.
[0019] Furthermore, the defoaming agent is polyether-modified silicone oil.
[0020] Preferably, the drying and curing temperature and time in step (4) are 80-100° C. and 20-30 min, respectively, and the cooling method in step (5) is air cooling.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention adds an acid-printing step on the basis of existing printing, which widens the pH value control range of the water-based ink during the printing process, facilitates operation, increases the pH value of the water-based ink, and can also reduce the viscosity of the water-based ink, improve fluidity, and help improve the smooth performance of inkjet;
[0023] 2. When the water-based ink printed on the printing substrate contacts the acid-printed material, due to the presence of the acid-base buffer, the pH value slowly decreases, and the viscosity of the water-based ink gradually increases, which can improve the drying efficiency and avoid uneven color of the printed body caused by too fast viscosity change; the viscosity of the water-based ink at the edge is faster and the drying efficiency is faster, which can avoid the problem of poor printing quality caused by the diffusion of water-based ink with good fluidity. At the same time, the improvement of drying efficiency can also reduce the drying time and temperature for the later drying, which plays a role in energy-saving production;
[0024] 3. Compared with traditional inkjet printing, the printing method provided by the present invention can greatly reduce Vocs pollution. DETAILED DESCRIPTION
[0025] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described below in conjunction with various embodiments. The implementation of the present invention includes but is not limited to the following embodiments.
[0026] Example 1
[0027] The water-based ink used in this embodiment is a commercially available product purchased from outside, the pH value of the dilute hydrochloric acid used is 3-5, and it is prepared by using ordinary hydrochloric acid, and the printing substrate used is a paper-plastic board.
[0028] Preparation of water-based ink before printing: Add water and glycine-sodium hydroxide buffer to dissolve the water-based ink, and control its pH value to 8-11, preferably 9.5-10.5.
[0029] The printing process is as follows:
[0030] (1) Cleaning the paper-plastic board: Clean the surface of the paper-plastic board to make it dust-free and keep it clean, and then fix it to the designated position;
[0031] (2) Acid printing: Use dilute hydrochloric acid instead of ink for printing. No specific pattern needs to be formed in this process. Just spray the dilute acid on the area to be printed.
[0032] (3) Spraying water-based ink: After positioning again, print the water-based ink onto the acidic printed matter of the paper-plastic board;
[0033] (4) Drying and curing: The printed paper-plastic board is transferred to a closed space, and the printed material C is dried and cured by an infrared drying device. The closed space is evacuated and ventilated before the device is turned on. The drying and curing temperature and time are 80-100° C. and 30 min, respectively. At this temperature, HCl can be released, and excess HCl is removed by evacuation and ventilation to avoid acid contamination.
[0034] (5) Cooling treatment: The dried and solidified product is transferred to a cooling room and cleaned and cooled by air cooling equipment. The printed product is obtained when it cools to room temperature.
[0035] Example 2
[0036] The water-based ink used in this embodiment is a commercially available product purchased from outside. The pH value of the dilute hydrochloric acid used is less than 1. It is prepared by using ordinary hydrochloric acid. The printing substrate used is a paper-plastic board.
[0037] Preparation of water-based ink before printing: Add water and glycine-sodium hydroxide buffer to dissolve the water-based ink, and control its pH value to 8-11, preferably 9.5-10.5.
[0038] The printing process is as follows:
[0039] (1) Cleaning the paper-plastic board: Clean the surface of the paper-plastic board to make it dust-free and keep it clean, and then fix it to the designated position;
[0040] (2) Acid printing: Use dilute hydrochloric acid instead of ink for printing. No specific pattern needs to be formed in this process. Just spray the dilute acid on the area to be printed.
[0041] (3) Spraying water-based ink: After positioning again, print the water-based ink onto the acidic printed matter of the paper-plastic board;
[0042] (4) Drying and curing: The printed paper-plastic board is transferred to a closed space, and the printed material C is dried and cured by an infrared drying device. The closed space is evacuated and ventilated before the device is turned on. The drying and curing temperature and time are 80-100° C. and 30 min, respectively. At this temperature, HCl can be released, and excess HCl is removed by evacuation and ventilation to avoid acid contamination.
[0043] (5) Cooling treatment: The dried and solidified product is transferred to a cooling room and cleaned and cooled by air cooling equipment. The printed product is obtained when it cools to room temperature.
[0044] Example 3
[0045] The water-based ink used in this embodiment is a commercially available product purchased from outside, the pH value of the dilute hydrochloric acid used is greater than 5, and it is prepared using ordinary hydrochloric acid, and the printing substrate used is a paper-plastic board.
[0046] Preparation of water-based ink before printing: Add water and glycine-sodium hydroxide buffer to dissolve the water-based ink, and control its pH value to 8-11, preferably 9.5-10.5.
[0047] The printing process is as follows:
[0048] (1) Cleaning the paper-plastic board: Clean the surface of the paper-plastic board to make it dust-free and keep it clean, and then fix it to the designated position;
[0049] (2) Acid printing: Use dilute hydrochloric acid instead of ink for printing. No specific pattern needs to be formed in this process. Just spray the dilute acid on the area to be printed.
[0050] (3) Spraying water-based ink: After positioning again, print the water-based ink onto the acidic printed matter of the paper-plastic board;
[0051] (4) Drying and curing: The printed paper-plastic board is transferred to a closed space, and the printed material C is dried and cured by an infrared drying device. The closed space is evacuated and ventilated before the device is turned on. The drying and curing temperature and time are 80-100° C. and 30 min, respectively. At this temperature, HCl can be released, and excess HCl is removed by evacuation and ventilation to avoid acid contamination.
[0052] (5) Cooling treatment: The dried and solidified product is transferred to a cooling room and cleaned and cooled by air cooling equipment. The printed product is obtained when it cools to room temperature.
[0053] Example 4
[0054] The water-based ink used in this embodiment is a commercially available product purchased from outside, the pH value of the dilute hydrochloric acid used is 3-5, and it is prepared by using ordinary hydrochloric acid, and the printing substrate used is a paper-plastic board.
[0055] Preparation of water-based ink before printing: Add water to dissolve the water-based ink, and control its pH value to 8-11, preferably 9.5-10.5, by adding acid and alkali reagents.
[0056] The printing process is as follows:
[0057] (1) Cleaning the paper-plastic board: Clean the surface of the paper-plastic board to make it dust-free and keep it clean, and then fix it to the designated position;
[0058] (2) Acid printing: Use dilute hydrochloric acid instead of ink for printing. No specific pattern needs to be formed in this process. Just spray the dilute acid on the area to be printed.
[0059] (3) Spraying water-based ink: After positioning again, print the water-based ink onto the acidic printed matter of the paper-plastic board;
[0060] (4) Drying and curing: The printed paper-plastic board is transferred to a closed space, and the printed material C is dried and cured by an infrared drying device. The closed space is evacuated and ventilated before the device is turned on. The drying and curing temperature and time are 80-100° C. and 30 min, respectively. At this temperature, HCl can be released, and excess HCl is removed by evacuation and ventilation to avoid acid contamination.
[0061] (5) Cooling treatment: The dried and solidified product is transferred to a cooling room and cleaned and cooled by air cooling equipment. The printed product is obtained when it cools to room temperature.
[0062] Example 5
[0063] The water-based ink used in this embodiment is a self-prepared product, and its specific ingredients are: 25 parts of pigment, 20 parts of water-soluble synthetic resin, 5 parts of glycerin, 5 parts of soybean oil, 6 parts of fatty acid methyl ester, 2 parts of magnesium stearate, 0.5 parts of tert-butylhydroquinone, and 0.5 parts of polyether modified silicone oil.
[0064] The pH value of the diluted hydrochloric acid used is 3-5, and it is prepared by using ordinary hydrochloric acid. The printing substrate used is a paper-plastic board.
[0065] Preparation of water-based ink before printing: Add water and glycine-sodium hydroxide buffer to dissolve the self-prepared water-based ink, and control its pH value to 8-11, preferably 9.5-10.5.
[0066] The printing process is as follows:
[0067] (1) Cleaning the paper-plastic board: Clean the surface of the paper-plastic board to make it dust-free and keep it clean, and then fix it to the designated position;
[0068] (2) Acid printing: Use dilute hydrochloric acid instead of ink for printing. No specific pattern needs to be formed in this process. Just spray the dilute acid on the area to be printed.
[0069] (3) Spraying water-based ink: After positioning again, print the water-based ink onto the acidic printed matter of the paper-plastic board;
[0070] (4) Drying and curing: The printed paper-plastic board is transferred to a closed space, and the printed material C is dried and cured by an infrared drying device. The closed space is evacuated and ventilated before the device is turned on. The drying and curing temperature and time are 80-100° C. and 30 min, respectively. At this temperature, HCl can be released, and excess HCl is removed by evacuation and ventilation to avoid acid contamination.
[0071] (5) Cooling treatment: The dried and solidified product is transferred to a cooling room and cleaned and cooled by air cooling equipment. The printed product is obtained when it cools to room temperature.
[0072] Example 6
[0073] The water-based ink used in this embodiment is a self-prepared product, and its specific ingredients are: 25 parts of pigment, 20 parts of water-soluble synthetic resin, 5 parts of glycerin, 5 parts of soybean oil, 6 parts of fatty acid methyl ester, 2 parts of magnesium stearate, 2 parts of drying agent (the drying agent is a mixture of cobalt cyclopentaneate and manganese cyclopentaneate in a weight ratio of 1:5), 0.5 parts of tert-butylhydroquinone, and 0.5 parts of polyether modified silicone oil.
[0074] The printing substrate used is paper-plastic board.
[0075] Preparation of water-based ink before printing: Add water and glycine-sodium hydroxide buffer to dissolve the self-prepared water-based ink, and control its pH value to 8-11, preferably 9.5-10.5.
[0076] The printing process is as follows:
[0077] (1) Cleaning the paper-plastic board: Clean the surface of the paper-plastic board to make it dust-free and keep it clean, and then fix it to the designated position;
[0078] (2) Spraying water-based ink: After positioning again, print the water-based ink onto the paper-plastic board;
[0079] (3) Drying and curing: The printed paper-plastic board is transferred to a closed space, and the printed material C is dried and cured by an infrared drying device. The closed space is evacuated and ventilated before the device is turned on. The drying and curing temperature and time are 80-100° C. and 30 min, respectively. At this temperature, HCl can be released, and excess HCl is removed by evacuation and ventilation to avoid acid contamination.
[0080] (4) Cooling treatment: The dried and solidified product is transferred to a cooling room and cleaned and cooled by air cooling equipment. The printed product is obtained when it is cooled to room temperature.
[0081] Example 7
[0082] The water-based ink used in this embodiment is a self-prepared product, and its specific ingredients are: 25 parts of pigment, 20 parts of water-soluble synthetic resin, 5 parts of glycerin, 5 parts of soybean oil, 6 parts of fatty acid methyl ester, 2 parts of magnesium stearate, 0.5 parts of tert-butylhydroquinone, and 0.5 parts of polyether modified silicone oil.
[0083] The printing substrate used is paper-plastic board.
[0084] Preparation of water-based ink before printing: Add water and glycine-sodium hydroxide buffer to dissolve the self-prepared water-based ink, and control its pH value to 8-11, preferably 9.5-10.5.
[0085] The printing process is as follows:
[0086] (1) Cleaning the paper-plastic board: Clean the surface of the paper-plastic board to make it dust-free and keep it clean, and then fix it to the designated position;
[0087] (2) Spraying water-based ink: After positioning again, print the water-based ink onto the paper-plastic board;
[0088] (3) Drying and curing: The printed paper-plastic board is transferred to a closed space, and the printed material C is dried and cured by an infrared drying device. The closed space is evacuated and ventilated before the device is turned on. The drying and curing temperature and time are 80-100° C. and 30 min, respectively. At this temperature, HCl can be released, and excess HCl is removed by evacuation and ventilation to avoid acid contamination.
[0089] (4) Cooling treatment: The dried and solidified product is transferred to a cooling room and cleaned and cooled by air cooling equipment. The printed product is obtained when it is cooled to room temperature.
[0090] Example 8
[0091] The water-based ink used in this embodiment is a self-prepared product, and its specific ingredients are: 25 parts of pigment, 20 parts of water-soluble synthetic resin, 5 parts of glycerin, 5 parts of soybean oil, 6 parts of fatty acid methyl ester, 2 parts of magnesium stearate, 2 parts of drying agent (the drying agent is a mixture of cobalt cyclopentaneate and manganese cyclopentaneate in a weight ratio of 1:5), 0.5 parts of tert-butylhydroquinone, and 0.5 parts of polyether modified silicone oil.
[0092] The pH value of the diluted hydrochloric acid used is 3-5, and it is prepared by using ordinary hydrochloric acid. The printing substrate used is a paper-plastic board.
[0093] Preparation of water-based ink before printing: Add water and glycine-sodium hydroxide buffer to dissolve the self-prepared water-based ink, and control its pH value to 8-11, preferably 9.5-10.5.
[0094] The printing process is as follows:
[0095] (1) Cleaning the paper-plastic board: Clean the surface of the paper-plastic board to make it dust-free and keep it clean, and then fix it to the designated position;
[0096] (2) Acid printing: Use dilute hydrochloric acid instead of ink for printing. No specific pattern needs to be formed in this process. Just spray the dilute acid on the area to be printed.
[0097] (3) Spraying water-based ink: After positioning again, print the water-based ink onto the acidic printed matter of the paper-plastic board;
[0098] (4) Drying and curing: The printed paper-plastic board is transferred to a closed space, and the printed material C is dried and cured by an infrared drying device. The closed space is evacuated and ventilated before the device is turned on. The drying and curing temperature and time are 80-100° C. and 30 min, respectively. At this temperature, HCl can be released, and excess HCl is removed by evacuation and ventilation to avoid acid contamination.
[0099] (5) Cooling treatment: The dried and solidified product is transferred to a cooling room and cleaned and cooled by air cooling equipment. The printed product is obtained when it cools to room temperature.
[0100] Example 9
[0101] The water-based ink used in this embodiment is a self-prepared product, and its specific ingredients are: 25 parts of pigment, 20 parts of water-soluble synthetic resin, 5 parts of glycerin, 5 parts of soybean oil, 6 parts of fatty acid methyl ester, 2 parts of magnesium stearate, 2 parts of drying agent (the drying agent is a mixture of cobalt cyclopentaneate and manganese cyclopentaneate in a weight ratio of 1:5), 0.5 parts of tert-butylhydroquinone, and 0.5 parts of polyether modified silicone oil.
[0102] The pH value of the diluted hydrochloric acid used is 3-5, and it is prepared by using ordinary hydrochloric acid. The printing substrate used is a paper-plastic board.
[0103] Preparation of water-based ink before printing: Add water and glycine-sodium hydroxide buffer to dissolve the self-prepared water-based ink, and control its pH value to 8-11, preferably 9.5-10.5.
[0104] The printing process is as follows:
[0105] (1) Cleaning the paper-plastic board: Clean the surface of the paper-plastic board to make it dust-free and keep it clean, and then fix it to the designated position;
[0106] (2) Acid printing: Use dilute hydrochloric acid instead of ink for printing. No specific pattern needs to be formed in this process. Just spray the dilute acid on the area to be printed.
[0107] (3) Spraying water-based ink: After positioning again, print the water-based ink onto the acidic printed matter of the paper-plastic board;
[0108] (4) Drying and curing: The printed paper-plastic board is transferred to a closed space, and the printed material C is dried and cured by an infrared drying device. The closed space is evacuated and ventilated before the device is turned on. The drying and curing temperature and time are 80-100° C. and 20 min, respectively. At this temperature, HCl can be released, and excess HCl is removed by evacuation and ventilation to avoid acid contamination.
[0109] (5) Cooling treatment: The dried and solidified product is transferred to a cooling room and cleaned and cooled by air cooling equipment. The printed product is obtained when it cools to room temperature.
[0110] The printed products obtained in Examples 1 to 9 were compared, and the comparison results are shown in Table 1.
[0111] Table 1
[0112] Product Group Uniform coloring of printed matter Whether the printed text is blurred Inkjet smoothness Is it dry? Example 1 Uniform No smudging Smooth dry Example 2 Uneven No smudging Smooth dry Example 3 Uniform Slight smudging Smooth Not dried Example 4 Uneven No smudging Smooth dry Example 5 Uniform No smudging Smooth dry Example 6 Uniform Slight smudging There is a phenomenon of nozzle blockage Not dried Example 7 Uniform Slight smudging Smooth Not dried Example 8 Uniform No smudging There is a phenomenon of nozzle blockage dry Example 9 Uniform No smudging There is a phenomenon of nozzle blockage dry
[0113] The above embodiment is only one of the preferred implementation modes of the present invention and should not be used to limit the protection scope of the present invention. Any changes or modifications that are made to the main design concept and spirit of the present invention and have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention.
Claims
1. A green, environmentally friendly, energy-saving water-based ink printing process, characterized in that: The steps include: (1) Cleaning the printing substrate A: Clean the surface of the printing substrate to make it dust-free and keep it clean, and then fix it to the designated position; (2) Acid printing: Use dilute acid instead of ink to print first to obtain printing substrate B; (3) Spraying water-based ink: After positioning again, print the water-based ink with a pH value ranging from 8 to 11 onto the acidic printed material of the printing substrate B to obtain the printed material C; the dilute acid solution is dilute hydrochloric acid with a pH value of 3 to 5, and its usage amount is 20% to 30% of the water-based ink used for printing; in this step, the pH value range of the water-based ink is controlled to 8 to 11 using a glycine-sodium hydroxide buffer with a pH value range of 8 to 11; The water-based ink comprises the following specific components by weight: 25 to 30 parts of pigment, 20 to 25 parts of water-soluble synthetic resin, 5 to 10 parts of glycerol, 5 to 10 parts of vegetable oil, 4 to 6 parts of fatty acid methyl ester, 2 to 3 parts of dispersant, 0.5 to 1 part of antioxidant, and 0.5 to 1 part of defoaming agent; (4) Drying and curing: In a confined space, the printed material C is dried and cured by infrared drying equipment, and the confined space is evacuated and ventilated before the equipment is turned on; (5) Cooling treatment: The dried and solidified product is transferred to a cooling room and cooled by refrigeration equipment. The printed product is obtained when it is cooled to room temperature.
2. The green, environment-friendly, energy-saving water-based ink printing process according to claim 1, characterized in that: The vegetable oil is one or more of soybean oil, corn oil, sunflower oil, tung oil and peanut oil.
3. The green, environment-friendly, energy-saving water-based ink printing process according to claim 1, characterized in that: The dispersant is a metal soap substance.
4. The green, environment-friendly, energy-saving water-based ink printing process according to claim 1, characterized in that: The antioxidant is one or more of tea polyphenols, tocopherol, flavonoids, butylated hydroxyanisole, butylated hydroxytoluene, and tert-butylhydroquinone.
5. The green, environment-friendly, energy-saving water-based ink printing process according to claim 1, characterized in that: The defoamer is polyether modified silicone oil.