A room temperature curing low color modified alicyclic amine curing agent and preparation method thereof
By controlling the reaction conditions under nitrogen protection conditions, a low-color modified alicyclic amine curing agent was generated, which solved the problem of slow curing and coloring of isophorone diamine and epoxy resin at room temperature, and achieved rapid curing and The effect of high light transmittance meets the production requirements of safety and environmental protection.
Patent Information
- Application Number
- CN202110894898.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-08-05
AI Technical Summary
In the prior art, isophorone diamine and epoxy resin cure slowly at room temperature and are easily affected by environmental humidity, resulting in unstable coatings, and chromogenic groups are easily generated during the preparation of commonly used modification curing agents. It is difficult to achieve clear and transparent effect, and the nonylphenol used at the same time has a carcinogenic risk and cannot meet safety and environmental protection requirements.
Under nitrogen protection conditions, the temperature and addition rate are controlled, and the benzyl alcohol solution containing monofunctional glycidyl ether is reacted with isophorone diamine to form a low-color modified alicyclic amine curing agent to avoid the addition of nonyl Phenol achieves rapid curing and high light transmittance at room temperature.
It realizes rapid curing of modified alicyclic amine curing agent at room temperature, has high light transmittance, flat surface, smoothness, and no whitening phenomenon, and is simple in preparation process and low in cost. It is suitable for large-scale production and meets environmental protection requirements.
Abstract
Description
Technical Field
[0001] The invention relates to a modified alicyclic amine curing agent and a preparation method thereof, in particular to a room temperature curing low color modified alicyclic amine curing agent obtained by modifying isophorone diamine with benzyl glycidyl ether or decyl glycidyl ether, and also to a preparation method thereof; the invention belongs to the technical field of modified alicyclic amine curing agents. Background Art
[0002] Epoxy resin is an important thermosetting plastic with excellent properties such as high bonding strength, small shrinkage, good dielectric properties and heat resistance. Epoxy resin alone has no practical application value and must be compounded with a curing agent before use. Adhesives using epoxy resin and amine curing agents are widely used in ornamental crystal glue and jewelry industries. Currently, commonly used room temperature curing agents include fatty amines: diethylenetriamine, triethylenetetramine and alicyclic polyamines: IPDA, AEP, etc.
[0003] Isophorone diamine IPDA is an excellent alicyclic amine with low color, low viscosity, high strength, good weather resistance and chemical resistance. It is currently widely used in ornamental potting products. IPDA reacts slowly with epoxy resin at room temperature and needs to be heated for curing. It is easily affected by environmental humidity when curing with epoxy resin at room temperature, absorbs moisture in the air, forms carbonates, and makes the coating surface sweat, turbid and opaque. The cured surface has problems such as whitening and orange peel, which leads to product instability. At present, epoxy group modification is generally used to reduce its reaction activity. The modified curing agent is easy to produce color-causing groups during the synthesis process. Therefore, it is difficult to achieve a clear and transparent effect when used for ornamental potting products. In addition, the existing patented technology for preparing modified alicyclic amine curing agents still needs to add nonylphenol during use to promote the curing reaction and increase the gloss and water permeability resistance of the cured product. Nonylphenol is an organic pollutant and a carcinogen. It can kill male sperm and promote the proliferation of breast cancer cells. It is extremely harmful to the body and cannot meet safety and environmental protection requirements. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a modified alicyclic amine curing agent that can be cured with epoxy resin at room temperature and has the characteristics of fast curing speed, light color of the cured system, resistance to whitening, etc. The modified curing agent can be used for ornamental potting products. It can be quickly cured with epoxy resin at room temperature without adding nonylphenol, and the surface of the cured product is flat, smooth and not whitish. At the same time, it can achieve a high light transmittance and has a crystal clear visual effect.
[0005] The second object of the present invention is to provide a method for preparing a modified alicyclic amine curing agent, which has simple operation, mild conditions, low cost and is conducive to large-scale production.
[0006] In order to achieve the above technical purpose, the present invention provides a method for preparing a room temperature curing low color modified alicyclic amine curing agent, the method comprising: adding a benzyl alcohol solution containing monofunctional glycidyl ether to a reactor containing a benzyl alcohol solution of isophorone diamine under nitrogen protection conditions to carry out a reaction, the addition rate of the benzyl alcohol solution containing monofunctional glycidyl ether is controlled to keep the temperature in the reactor below 60°C, after the benzyl alcohol solution containing monofunctional glycidyl ether is added, evacuating the reactor and keeping the temperature in the reactor at 60-70°C to carry out the reaction, and after the reaction is completed, cooling and discharging the material to obtain the curing agent.
[0007] As a preferred solution, the monofunctional glycidyl ether is benzyl glycidyl ether and / or decyl glycidyl ether. The preferred monofunctional glycidyl ether can control the reactivity of the hydroxyl group of the modified fatty amine curing agent.
[0008] As a preferred solution, the mass ratio of monofunctional glycidyl ether, isophorone diamine and benzyl alcohol is 30-35:45-50:10-20. Benzyl alcohol is used as an inactive diluent, which can well dissolve monofunctional glycidyl ether and isophorone diamine raw materials and the generated modified alicyclic amine curing agent, and is also used to adjust the viscosity of the modified curing agent. Monofunctional glycidyl ether is mainly used as a modifying agent for isophorone diamine. Monofunctional glycidyl ether reacts with the active amino group in isophorone diamine through its epoxy group to generate an adduct with an increased molecular weight, a reduced free amine, and a reduced polarity, thereby improving the curing water stain resistance. At the same time, the modified alicyclic amine curing agent modified with special monofunctional glycidyl ether has improved activity, can achieve rapid curing at room temperature, and can solve the technical problems of incomplete curing of fatty amine curing agents at room temperature and easy whitening of the surface. The amount of monofunctional glycidyl ether will affect the viscosity and amine value of the modified alicyclic amine curing agent, so it is necessary to maintain a suitable dosage ratio to obtain the modified alicyclic amine curing agent with the best performance.
[0009] As a preferred solution, the benzyl alcohol solution of isophoronediamine in the reaction kettle is preheated to 40-60°C.
[0010] As a preferred solution, the rate of adding the benzyl alcohol solution of monofunctional glycidyl ether controls the temperature in the reactor to be between 50 and 60° C. If the reaction temperature is too low, the modification reaction will be incomplete, and if the temperature is too high, the color of the product will be affected.
[0011] As a preferred solution, the benzyl alcohol solution of monofunctional glycidyl ether is added slowly and continuously or in multiple batches, for example, in three batches of 40%, 30%, and 30%, or slowly and continuously.
[0012] As a preferred solution, the reactor is evacuated to a vacuum degree of 50-70 kPa. Evacuation and control under appropriate vacuum conditions can protect the reaction and reduce the oxygen content in the reaction system. On the other hand, evacuation can take away heat and slow down the temperature rise of the system caused by the exothermic reaction, thereby ensuring the low color of the product.
[0013] As a preferred embodiment, the reaction time is 1 to 3 hours at 60 to 70°C.
[0014] The present invention also provides a room temperature curing low color modified alicyclic amine curing agent, which is obtained by the preparation method.
[0015] As a preferred solution, the color number of the modified alicyclic amine curing agent is less than 15, and the amine value measured by the platinum-cobalt method is 250 mg KOH / g to 350 mg KOH / g, and the active hydrogen equivalent is 90 g / eq to 120 g / eq.
[0016] The present invention provides a method for preparing a room temperature curing low color modified alicyclic amine curing agent, comprising the following specific steps:
[0017] 1) In a reactor with a stirring device, add 30-35 parts of glycidyl ether and 10 parts of benzyl alcohol, start the stirrer, and stir the materials evenly at low temperature (<40° C.) for standby use;
[0018] 2) In a reactor with a stirring device, 45-50 parts of isophorone diamine (IPDA) and the remaining benzyl alcohol are added, and then the stirrer is started to heat the materials to 40-50° C.; the materials obtained by mixing in the first step are added through a peristaltic pump for reaction, and the addition speed is controlled so that the reaction temperature is maintained below 60° C. The addition of the modified glycidyl ether is completed within 1.5 hours, and nitrogen protection is passed through the system during the addition of the modifier;
[0019] 3) Raise the stirring speed to 200 r / m, carry out the reaction for 1 to 3 hours under the conditions of vacuum degree of 50 to 70 KPa and temperature of 60 to 70° C., cool and discharge the material after the reaction is completed, and obtain a modified alicyclic amine curing agent.
[0020] The modified alicyclic amine curing agent prepared by the invention has a color number of less than 15 (platinum-cobalt method), an amine value of 250-350 mgKOH / g, and a viscosity of 300-500 (25° C., mpa.s).
[0021] The room temperature curing low color modified alicyclic amine curing agent of the present invention has the characteristics of light color, high gloss, moisture resistance, environmental protection and the like, and can be used alone or compounded with other amine curing agents to be used as a curing agent for ornamental potting glue and crystal glue for ornaments.
[0022] The modified alicyclic amine curing agent of the present invention is prepared by controlling the reaction temperature and the atmosphere of the reaction system to achieve low color of the product. By controlling the reaction at a low temperature, the reaction can be made more uniform, the chain growth of the reaction can be effectively controlled, and the generation of auxochrome groups is not conducive. At the same time, nitrogen protection and vacuuming can also effectively prevent oxidation reactions and temperature mutations from causing unstable reactions and generating chromogenic groups.
[0023] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:
[0024] The modified alicyclic amine curing agent prepared by the invention has a color number of less than 15 (platinum-cobalt method), an amine value of 250-350 mg KOH / g, and a viscosity of 300-500 (25° C., mpa.s).
[0025] The modified alicyclic amine curing agent prepared by the invention has the characteristics of light color, high gloss, moisture resistance, environmental protection and the like, and can be used alone or compounded with other amine curing agents to be used as a curing agent for ornamental potting glue and crystal glue for ornaments.
[0026] The modified alicyclic amine curing agent prepared by the present invention is mixed and cured with epoxy epoxy in an equivalent amount, and the cured product has the following characteristics: 1) fast room temperature curing speed, the gel time of the modified curing agent and the equivalent epoxy resin mixed is 50-70 minutes; 2) high hardness, after three days of curing at room temperature, the Shore hardness is greater than 75D; 3) high light transmittance. After three days of curing at room temperature, the light transmittance of the cured product is greater than 95%; 4) low shrinkage, the system curing shrinkage does not exceed 1%.
[0027] The preparation method of the modified alicyclic amine curing agent prepared by the invention has readily available raw materials, low cost, simple process steps and is conducive to large-scale production and application. DETAILED DESCRIPTION
[0028] In order to better understand the present invention, the present invention is further described in detail in conjunction with embodiments, but the scope of the present invention is not limited to the scope represented by the embodiments.
[0029] The chemical raw materials involved in the following examples are all common commercially available raw materials unless otherwise specified.
[0030] Product performance testing methods are all industry standards.
[0031] Example 1
[0032] In a four-necked flask with a stirrer, add 34 parts of benzyl glycidyl ether and 10 parts of benzyl alcohol. At room temperature, start the stirrer and stir the materials evenly for standby use. In a four-necked flask with a stirring device and a thermometer, add 46 parts of isophorone diamine (IPDA) and 10 parts of benzyl alcohol, then start the stirrer and heat the materials to 50°C; the mixed modified product obtained in the first step is continuously added to the reactor through a peristaltic pump for reaction, and the rate of adding the modifier is controlled so that the reaction temperature is maintained below 60°C. Nitrogen protection is passed during the addition of the modifier. After the addition of the modifier is completed, the reaction pressure is controlled at 50-60kPa by a vacuum circulation pump, and the temperature is raised to 60°C for reaction for 2h. The obtained product is: Appearance: colorless and transparent liquid; Color number (platinum cobalt method) 12; Amine value (mgKOH / g) 309; Active hydrogen equivalent (g / eq) 115. The amount of curing agent used for 100 grams of standard epoxy resin (EEW=190g / eq) is 55 grams; the modified alicyclic amine curing agent and epoxy resin E-51 are mixed in proportion for curing, and the room temperature curing gel time is 68 minutes; the cured product has uniform color, smooth surface, no whitening phenomenon, Shore hardness reaches 77D, transmittance: 96%, and shrinkage rate <1%.
[0033] Example 2
[0034] In a three-necked flask with a stirrer, add 30 parts of decyl glycidyl ether and 8 parts of benzyl alcohol. At room temperature, start the stirrer and stir the materials evenly for use. In a four-necked flask with a stirring device, a constant pressure dropping funnel and a thermometer, add 50 parts of isophorone diamine (IPDA) and 7 parts of benzyl alcohol, then start the stirrer and heat the materials to 40°C; slowly add the mixed modified product obtained in the first step to the four-necked flask through the dropping funnel for reaction, and add it three times. The first time, add 40% of the total amount, maintain stirring for 0.5h, and then add 30% and 30% respectively. Nitrogen protection is passed during the addition of the modifier, and the temperature is maintained below 60°C. After the addition is completed, the temperature is raised to 67°C and the pressure is 60-70kPa for reaction for 2h. The obtained product has the appearance: colorless and transparent liquid; color number (platinum cobalt method): 10; amine value (mgKOH / g) 350; active hydrogen equivalent (g / eq) 91. The amount of curing agent used is 50 grams per 100 grams of standard epoxy resin (EEW = 190g / eq). The modified alicyclic amine curing agent and epoxy resin E-51 are mixed and cured in proportion. The room temperature curing gel time is 54 minutes. The cured product has uniform color, smooth surface, no whitening phenomenon, Shore hardness reaches 86D, high transparency: 96%, and shrinkage rate <1%.
[0035] Example 3
[0036] In a three-necked flask with a stirrer, add 32 parts of a mixture of benzyl glycidyl ether and decyl glycidyl ether and 10 parts of benzyl alcohol. At room temperature, start the stirrer and stir the materials evenly for standby use. In a four-necked flask with a stirring device and a thermometer, add 48 parts of isophorone diamine (IPDA) and 7 parts of benzyl alcohol, then start the stirrer and heat the materials to 40°C; slowly drip the mixed modified product obtained in the first step into the four-necked flask through a peristaltic pump for reaction, control the rate of adding the modifier so that the reaction temperature is maintained below 60°C, and pass nitrogen protection at the same time, and complete the dripping within 1.5h. After the dripping is completed, heat to 69°C, and react at a pressure of 55-65kPa for 2h. The obtained product is: Appearance: colorless and transparent liquid; Color number (platinum cobalt method): 13; Amine value (mgKOH / g) 297; Active hydrogen equivalent (g / eq) 99. The amount of curing agent used for 100 grams of standard epoxy resin (EEW = 190g / eq) is 54 grams; the modified alicyclic amine curing agent and epoxy resin E-51 are mixed and cured in proportion, and the room temperature curing gel time is 61 minutes; the cured product has uniform color, smooth surface, no whitening phenomenon, Shore hardness reaches 80D, high transparency: 96%; low shrinkage rate <1%.
[0037] Example 4
[0038] In a four-necked flask with a stirrer, add 34 parts of benzyl glycidyl ether and 10 parts of benzyl alcohol. At room temperature, start the stirrer and stir the materials evenly for standby use. In a four-necked flask with a stirring device and a thermometer, add 46 parts of isophorone diamine (IPDA) and 10 parts of benzyl alcohol, then start the stirrer and heat the materials to 50°C; the mixed modified product obtained in the first step is continuously added to the reactor through a peristaltic pump for reaction, and the rate of adding the modifier is controlled so that the reaction temperature is maintained below 60°C. Nitrogen protection is passed during the addition of the modifier. After the addition of the modifier is completed, the reaction temperature is controlled at 80°C for 2h. The obtained product is: Appearance: yellow transparent liquid; Color number (platinum cobalt method) 32; Amine value (mgKOH / g) 315. The amount of curing agent used for 100 grams of standard epoxy resin (EEW=190g / eq) is 55 grams. The modified alicyclic amine curing agent and epoxy resin E-51 are mixed in proportion for curing, and the room temperature curing gel time is 54 minutes; the cured product is yellow in color, with a smooth and flat surface without whitening, a Shore hardness of 77D, a transmittance of 94%, and a shrinkage rate of <1%.
[0039] Comparative Example 1
[0040] In a three-necked flask with a stirrer, add 30 parts of decyl glycidyl ether and 8 parts of benzyl alcohol. At room temperature, start the stirrer and stir the materials evenly for standby use. In a four-necked flask with a stirring device, a constant pressure dropping funnel and a thermometer, add 50 parts of isophorone diamine (IPDA) and 7 parts of benzyl alcohol, then start the stirrer and heat the materials to 40°C; add the mixed modified product obtained in the first step to the reactor at one time and maintain stirring for 0.5h. After the addition is completed, heat to 70°C and react at a pressure of 60-70kPa for 4h. The obtained product is: Appearance: light yellow transparent liquid; Color number (platinum cobalt method): 36; Amine value (mgKOH / g): 347; Active hydrogen equivalent (g / eq): 91.
[0041] The amount of curing agent used is 50 grams per 100 grams of standard epoxy resin (EEW = 190g / eq). The modified alicyclic amine curing agent and epoxy resin E-51 are mixed and cured in proportion. The room temperature curing gel time is 54 minutes. The cured product has uniform color, smooth surface, no whitening phenomenon, Shore hardness reaches 76D, transparency: 91%, and shrinkage rate <1%.
Claims
1. A method for preparing a room temperature curing low color modified alicyclic amine curing agent, characterized in that: Under nitrogen protection, a benzyl alcohol solution containing monofunctional glycidyl ether is added to a reactor containing a benzyl alcohol solution of isophorone diamine for reaction, the addition rate of the benzyl alcohol solution containing monofunctional glycidyl ether is controlled to keep the temperature in the reactor below 60° C. After the benzyl alcohol solution containing monofunctional glycidyl ether is added, the reactor is evacuated and the temperature in the reactor is kept at 60-70° C. for reaction, and after the reaction is completed, the temperature is lowered and the material is discharged to obtain; The monofunctional glycidyl ether is benzyl glycidyl ether and / or decyl glycidyl ether; The mass ratio of monofunctional glycidyl ether, isophorone diamine and benzyl alcohol is 30-35:45-50:10-20; The reactor is evacuated to a vacuum degree of 50-70 kPa.
2. The method for preparing a room temperature curing low color modified alicyclic amine curing agent according to claim 1, characterized in that: The benzyl alcohol solution of isophorone diamine in the reaction kettle is preheated to 40-60°C.
3. The method for preparing a room temperature curing low color modified alicyclic amine curing agent according to claim 1, characterized in that: The addition rate of the benzyl alcohol solution containing monofunctional glycidyl ether controls the temperature in the reactor at 50-60°C.
4. The method for preparing a room temperature curing low color modified alicyclic amine curing agent according to claim 1 or 3, characterized in that: The benzyl alcohol solution containing monofunctional glycidyl ether is added slowly and continuously or in batches.
5. The method for preparing a room temperature curing low color modified alicyclic amine curing agent according to claim 1, characterized in that: The reaction time is 1 to 3 hours at 60 to 70°C.
6. A room temperature curing low color modified alicyclic amine curing agent, characterized in that: Obtained by the preparation method according to any one of claims 1 to 5.
7. A room temperature curing low color modified alicyclic amine curing agent according to claim 6, characterized in that: The color number is less than 15, measured by the platinum-cobalt method, the amine value is 250 mg KOH / g ~350 mg KOH / g, and the active hydrogen equivalent is 90 g / eq ~120 g / eq.
Citation Information
Patent Citations
Epoxy adhesive for stone repairing and preparation method of epoxy adhesive
CN107916084A
Adducts of aromatic monoepoxy compounds and norbornanediamine