A method for cleaning graphite oxide without involving hydrochloric acid
Through the graphite oxide cleaning method without hydrochloric acid, the combination of sulfuric acid and hydrogen peroxide is used to solve the environmental protection and equipment corrosion problems caused by hydrochloric acid, the cleaning efficiency and purity of graphene oxide are improved, and it is suitable for industrial production.
Patent Information
- Application Number
- CN202111268446.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-10-29
AI Technical Summary
The use of hydrochloric acid during the cleaning process of existing graphite oxides and graphene oxides causes environmental protection problems, equipment corrosion and cleaning efficiency, and chloride ion residues limit their application in the electronics field.
The graphite oxide cleaning method is adopted that does not involve hydrochloric acid. The graphite is oxidized by chemical method and then diluted with water. Residual sulfuric acid is used to provide an acidic environment. It is cleaned multiple times in combination with hydrogen peroxide to improve the degree of hydrolysis and impurity elution efficiency, and reduce the generation of wastewater.
It effectively reduces the generation of wastewater, improves cleaning efficiency, reduces impurity residues, avoids hydrochloric acid pollution and equipment corrosion, and is suitable for the industrial production of graphene oxide materials.
Smart Images

Figure CN116062749B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of graphene manufacturing, and in particular provides a method for cleaning graphite oxide or graphene oxide without involving hydrochloric acid. Background Art
[0002] Graphene oxide is an important derivative of graphene and is often used as a precursor for preparing graphene. It is manufactured on a large scale because of its rich functional groups and good water solubility, and is used in the fields of thermal conductivity, energy storage, catalysis, medicine, etc. Graphene oxide is an intermediate in the production process of graphene oxide and is a form of graphene oxide that has not been hydrolyzed and peeled off to form a single layer.
[0003] The main preparation method of graphite oxide is the Hummers method: first, flake graphite or expanded graphite is intercalated and oxidized using an intercalator and an oxidant to obtain graphite oxide. Next, the graphite oxide is graphitized, cleaned, and filtered to collect the solid product. Finally, it is exfoliated into graphene oxide by ultrasound, shear stirring, high-pressure homogenization, etc. to form a dispersion.
[0004] In the process of cleaning and filtering graphite oxide, hydrochloric acid is often used as an additive. The main purpose of adding hydrochloric acid is: if potassium permanganate is used as an oxidant, hydrochloric acid can maintain an acidic environment to prevent the unreacted permanganate ions from reacting with low-valent manganese ions to form manganese dioxide that is insoluble in water and difficult to elute; reduce the degree of hydrolysis and exfoliation of graphite oxide into graphene oxide, making it easier to separate and recover the solid from the liquid.
[0005] However, the introduction of hydrochloric acid also brings various environmental problems: the treatment of hydrochloric acid mist during the manufacturing process; the corrosion of metal parts in manufacturing equipment by hydrochloric acid; the problem of low hydrolysis degree cleaning reducing cleaning efficiency and generating more washing wastewater, etc. In addition to environmental issues, the residual chloride ions in graphite oxide and graphene oxide will also greatly limit their application in the electronics field.
[0006] Therefore, how to efficiently clean graphite oxide or graphene oxide without using hydrochloric acid is a problem that needs to be solved urgently in the current field. Summary of the invention
[0007] The purpose of the present invention is to provide a method for efficiently cleaning graphite oxide and graphene oxide without using hydrochloric acid, thereby reducing wastewater generation, improving production efficiency, and eliminating the adverse effects of hydrochloric acid.
[0008] The technical solution of the present invention is:
[0009] A method for cleaning graphite oxide without involving hydrochloric acid, wherein graphite is chemically oxidized to obtain a mixture of graphite oxide, an oxidant, an intercalating agent and other reaction products, which is diluted with water and then solid-liquid separated to collect a filter cake; the filter cake is washed with water to obtain a filter cake with higher purity, and then water and hydrogen peroxide are added to slurry and solid-liquid separated to obtain a high-purity graphite oxide filter cake.
[0010] The graphite oxide cleaning method not involving hydrochloric acid, the chemical graphite oxidation is a reaction system in which graphite, an intercalant, and an oxidant are mixed, the mass ratio of graphite to oxidant is in the range of 0.1 to 1, the mass ratio of graphite to intercalant is in the range of 0.01 to 0.1, the oxidant includes but is not limited to one or a combination of two or more of potassium permanganate, potassium chlorate, and sodium nitrate, the intercalant includes but is not limited to one or a combination of concentrated phosphoric acid and concentrated sulfuric acid, the concentration of concentrated sulfuric acid is 70 to 98wt%, and the concentration of concentrated phosphoric acid is ≥70wt%.
[0011] The graphite oxide cleaning method not involving hydrochloric acid, graphite includes but is not limited to one or a mixture of two or more of flake graphite, spherical graphite, and expanded graphite, the flake graphite has a diameter range of 30 to 5000 mesh, the spherical graphite has a particle size range of 30 to 5000 mesh, and the expanded graphite has a particle size range of 30 to 5000 mesh.
[0012] In the graphite oxide cleaning method not involving hydrochloric acid, when water is added for dilution, the mass ratio of graphite to water is in the range of 0.001 to 0.1.
[0013] The graphite oxide cleaning method not involving hydrochloric acid and the solid-liquid separation and filter cake collection method include but are not limited to one or a combination of two or more methods of centrifugation, filter pressing and suction filtration.
[0014] The graphite oxide cleaning method that does not involve hydrochloric acid, in the process of centrifugal collection of filter cake, the centrifugal speed is 1000rpm~12000rpm, and the centrifugal time is 10min~30min; in the process of filter cake collection by pressure filtration, the filter cloth material used includes but is not limited to: polyethersulfone, nylon, polyester or polycarbonate, the pore size of the filter cloth is 100 mesh~5000 mesh, the filter plate and filter frame material used include but are not limited to: stainless steel, polypropylene, polyethylene or polytetrafluoroethylene, the filter pressing equipment includes but is not limited to: bell filter press, plate and frame filter press, diaphragm filter press or hydraulic press, and the pressure range used is 0.1MPa~20MPa; in the process of suction filtration collection of filter cake, the filter membrane material used includes but is not limited to: polyethersulfone, nylon, polyester, mixed cellulose or polycarbonate, and the filter membrane pore size is 0.1μm~20μm.
[0015] In the graphite oxide cleaning method not involving hydrochloric acid, when the filter cake is cleaned with water, the cleaning times range from 1 to 5 times.
[0016] In the graphite oxide cleaning method not involving hydrochloric acid, when water and hydrogen peroxide are added for slurrying, the mass fraction of hydrogen peroxide in the hydrogen peroxide is in the range of 10% to 30%, the mass ratio of graphite to water is in the range of 0.001 to 0.1, and the mass ratio of graphite to hydrogen peroxide is in the range of 0.01 to 1.
[0017] In the graphite oxide cleaning method not involving hydrochloric acid, the solid mass fraction of the high-purity graphite oxide filter cake is 10-50%, and the impurity mass fraction is less than 0.5%.
[0018] The technical principle of the present invention is:
[0019] (1) Without using hydrochloric acid, residual sulfuric acid is used to provide an acidic environment to prevent unreacted potassium permanganate from chemically reacting with low-valent manganese ions to form manganese dioxide that is difficult to elute;
[0020] (2) Solid-liquid separation and collection of filter cakes minimizes the generation of wastewater;
[0021] (3) As the number of cleanings increases, the concentration of sulfuric acid decreases, and the uneluted potassium permanganate needs to be reduced with hydrogen peroxide to prevent the formation of manganese dioxide;
[0022] (4) Hydrogen peroxide is added to the relatively pure filter cake to cause the graphite oxide to undergo violent hydrolysis. The intercalated substances, such as sulfuric acid, intercalated between the graphite oxide layers will be released from the graphite oxide layers and dissolved in water. After solid-liquid separation and collection of the filter cake, a high-purity graphene oxide filter cake can be obtained.
[0023] The advantages and beneficial effects of the present invention are as follows:
[0024] 1. The present invention eliminates the pollution of hydrochloric acid to the environment and the corrosion of metal parts in the production equipment.
[0025] 2. The amount of washing wastewater generated by the present invention is low, and the mass ratio of graphite to wastewater can be controlled to be as low as 1:40.
[0026] 3. After adding hydrogen peroxide, the hydrolysis degree is increased, the intercalation agent and oxidant between the graphite oxide layers can be eluted more efficiently, and the impurity content remaining after cleaning is lower.
[0027] 4. The method of the present invention has the characteristics of high filter cake cleaning and collection efficiency, and no chloride ions in the cleaning wastewater and graphite oxide filter cake, and can be used for the industrial production of graphene oxide materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification sheet. They are used to explain the present invention together with the embodiments of the present invention, but are not used to limit the scope of the present invention.
[0029] Figure 1 .Scanning electron microscope photo of graphene oxide after cleaning and peeling using the method of the present invention.
[0030] Figure 2 .Atomic force microscope photograph of graphene oxide after cleaning and peeling using the method of the present invention.
[0031] Figure 3 . Raman spectrum of graphene oxide after cleaning and stripping using the method of the present invention. In the figure, the horizontal axis RamanShift represents the Raman shift (cm -1 ), the vertical axis Intensity represents the relative intensity (au). DETAILED DESCRIPTION
[0032] In the specific implementation process, the present invention does not involve a method for cleaning graphite oxide with hydrochloric acid. A chemical method is used to prepare graphite oxide. After the oxidation reaction is completed, a mixture of graphite oxide, intercalating agent, oxidant and other reaction products is diluted with water and then solid-liquid separation is performed to collect the filter cake; the filter cake is washed with water several times to obtain a filter cake with higher purity, and then water and hydrogen peroxide are added to slurry and solid-liquid separation is performed to obtain a high-purity graphite oxide filter cake.
[0033] The embodiments described in this specification are to further describe the specific implementation methods of the present invention in detail. The following embodiments are used to illustrate the present invention but are not used to limit the scope of the present invention.
[0034] Example 1.
[0035] In this embodiment, the mass of the flake graphite is 2 g, the diameter of the flake graphite is in the range of 300 to 500 meshes, and the graphite is chemically oxidized to obtain a mixture of oxidized graphite, sulfuric acid, sulfate, and manganate. The chemically oxidized graphite is a reaction system in which graphite, concentrated sulfuric acid, and potassium permanganate are mixed, wherein potassium permanganate is an oxidant and concentrated sulfuric acid is an intercalant. The mass ratio of graphite to potassium permanganate is 0.3, the mass ratio of graphite to concentrated sulfuric acid is 0.03, and the concentration of concentrated sulfuric acid is 98 wt%.
[0036] Add 30g of deionized water to the mixture of graphite oxide, sulfuric acid, sulfate, and manganate obtained after the reaction, stir slowly and evenly in an ice bath, control the solution temperature to be lower than 60°C, and the solution at this time is dark brown. Pour the solution into a bell filter press, pneumatically pressurize 0.5MPa, and press until no liquid flows out. Collect the filter cake and add 30g of deionized water, stir slowly and evenly, and the solution is dark brown at this time. Pour the solution into a bell filter press, pneumatically pressurize 0.5MPa, and press until no liquid flows out. Collect the filter cake and add 3g of hydrogen peroxide with a concentration of 30wt% and 27g of deionized water. The solution instantly releases a large amount of gas, and the color changes from dark brown to bright yellow. No gas is released after stirring evenly. Pour the solution into a bell filter press, pneumatically pressurize 0.5MPa, and press until no liquid flows out. Collect the filter cake. The solid mass fraction of graphite oxide in the filter cake is 40%, and the mass fraction of impurities is 0.08%.
[0037] In this example, a total of 120 g of filtrate was collected.
[0038] The conductivity of the obtained filter cake after dilution, shearing and peeling was 1600 μS / cm when the solid content was 2 wt%. The characterization results of scanning electron microscopy, atomic force microscopy and Raman spectroscopy are shown in Figure 1 , Figure 2 , Figure 3 .Depend on Figure 1 , Figure 2 , Figure 3 It can be seen that the diameter of the graphene oxide sheets cleaned by this method is 3 to 10 μm.
[0039] Example 2.
[0040] In this embodiment, the feed mass of flake graphite is 10 kg, the diameter range of flake graphite is 1000-2000 mesh, and the graphite is chemically oxidized to obtain a mixture of oxidized graphite, sulfuric acid, sulfate, and manganate. The chemically oxidized graphite is a reaction system in which graphite, concentrated sulfuric acid, and potassium permanganate are mixed, wherein potassium permanganate is an oxidant, and concentrated sulfuric acid is an intercalant. The mass ratio of graphite to potassium permanganate is 0.15, the mass ratio of graphite to concentrated sulfuric acid is 0.01, and the concentration of concentrated sulfuric acid is 98wt%.
[0041] Add 200kg of deionized water to the mixture of graphite oxide, sulfuric acid, sulfate, and manganate obtained after the reaction, stir slowly and evenly in a jacketed reactor, set the circulating cooling water at 15°C, and control the solution temperature below 60°C. The solution is dark brown at this time. Pump the solution into a diaphragm filter press with a diaphragm pump, pump pressure 0.6MPa, start oil pressure pressing after feeding, pressure 2MPa, press until no liquid flows out. Collect the filter cake and add 20kg of deionized water, slowly stir evenly in a stirring tank, and the solution is dark brown at this time. Pump the solution into a diaphragm filter press with a diaphragm pump, pump pressure 0.6MPa, start oil pressure pressing after feeding, pressure 2MPa, press until no liquid flows out. Collect the filter cake and add 10kg of hydrogen peroxide with a concentration of 30wt% and 100kg of deionized water. The solution instantly releases a large amount of gas, and the color changes from dark brown to bright yellow. No gas is released after stirring evenly in a stirring tank. The solution was pumped into the diaphragm filter press by a diaphragm pump at a pump pressure of 0.6 MPa. After the feeding was completed, the oil pressure was turned on at a pressure of 2 MPa until no liquid flowed out. The filter cake was collected. The mass fraction of graphite oxide solids in the filter cake was 35%, and the mass fraction of impurities was 0.06%.
[0042] In this example, a total of 90 kg of filtrate was collected.
[0043] The conductivity of the obtained filter cake after dilution, shearing and peeling was 1800 μS / cm when the solid content was 2 wt%.
[0044] Example 3.
[0045] In this embodiment, the feed mass of spherical graphite is 1g, the particle size range of spherical graphite is 300-600 mesh, and the graphite is chemically oxidized to obtain a mixture of oxidized graphite, phosphoric acid, phosphate, and manganate. The chemically oxidized graphite is a reaction system in which graphite, concentrated phosphoric acid, and potassium permanganate are mixed, wherein potassium permanganate is an oxidant, concentrated phosphoric acid is an intercalant, the mass ratio of graphite to potassium permanganate is 0.2, the mass ratio of graphite to concentrated phosphoric acid is 0.06, and the concentration of concentrated phosphoric acid is 75wt%.
[0046] Add 15g of deionized water to the mixture of graphite oxide, phosphoric acid, phosphate, and manganate obtained after the reaction, stir slowly and evenly in an ice bath, control the solution temperature to be lower than 60°C, and the solution is dark brown at this time. Pour the solution into a filter cup, filter at a pressure of -0.1MPa, and press until no liquid flows out. Collect the filter cake and add 15g of deionized water, stir slowly and evenly, and the solution is dark brown at this time. Pour the solution into a filter cup, filter at a pressure of -0.1MPa, and press until no liquid flows out. Collect the filter cake and add 1g of hydrogen peroxide with a concentration of 30wt% and 14g of deionized water. The solution instantly releases a large amount of gas, and the color changes from dark brown to bright yellow. No gas is released after stirring evenly. Pour the solution into a filter cup, filter at a pressure of -0.1MPa, and press until no liquid flows out. Collect the filter cake. The solid mass fraction of graphite oxide in the filter cake is 25%, and the mass fraction of impurities is 0.09%.
[0047] In this example, a total of 60 g of filtrate was collected.
[0048] The conductivity of the obtained filter cake after dilution, shearing and peeling was 1600 μS / cm when the solid content was 2 wt%.
[0049] Example 4.
[0050] In the present embodiment, the feed mass of expanded graphite is 1g, the particle size range of expanded graphite is 300-500 meshes, and graphite is chemically oxidized to obtain a mixture of graphite oxide, phosphoric acid, phosphate, and chloride. The chemically oxidized graphite is a reaction system in which graphite, concentrated phosphoric acid, and potassium chlorate are mixed, wherein potassium chlorate is an oxidant, and concentrated phosphoric acid is an intercalant. The mass ratio of graphite to potassium chlorate is 0.65, the mass ratio of graphite to concentrated phosphoric acid is 0.04, and the concentration of concentrated phosphoric acid is 70wt%.
[0051] Weigh the mixture of graphite oxide, phosphoric acid, phosphate, and chloride obtained at the end of the reaction, add 20g of deionized water, stir slowly and evenly in an ice bath, control the solution temperature to be below 60°C, and the solution is dark brown at this time. Pour the solution into a centrifuge tube and centrifuge at 12000rpm for 10min. Collect the precipitate and add 20g of deionized water, stir slowly and evenly, and the solution is dark brown at this time. Pour the solution into a centrifuge tube and centrifuge at 12000rpm for 10min. Repeat twice. Collect the precipitate and add 3g of hydrogen peroxide with a concentration of 30wt% and 17g of deionized water. The solution instantly releases a large amount of gas, and the color changes from dark brown to bright yellow. No gas is released after stirring evenly. Pour the solution into a centrifuge tube, centrifuge at 12000rpm for 10min, collect the precipitate, and the solid mass fraction of graphite oxide in the filter cake is 20%, and the mass fraction of impurities is 0.1%.
[0052] In this example, a total of 100 g of filtrate was collected.
[0053] The conductivity of the obtained filter cake after dilution, shearing and peeling was 1800 μS / cm when the solid content was 2 wt%.
[0054] The above results show that the method for cleaning graphite oxide without hydrochloric acid is simple and efficient, produces less washing wastewater, and has a good ion elution effect. More importantly, it solves the harm of hydrochloric acid mist to the human body, the pollution to the natural environment, and the corrosion to industrial equipment, and has high practical value.
[0055] The above embodiments are further explanations of the present invention, and the solid-liquid separation method therein can be subjected to several changes and improvements. Such changes and improvements in the process without departing from the technical process of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for cleaning graphite oxide without using hydrochloric acid, characterized in that: The graphite is chemically oxidized to obtain a mixture of graphite oxide, oxidant, intercalant and other reaction products, which is diluted with water and then solid-liquid separated to collect the filter cake; the filter cake is washed with water to obtain a filter cake with higher purity, and then water and hydrogen peroxide are added to slurry and solid-liquid separated to obtain a high-purity graphite oxide filter cake; Chemically oxidized graphite is a reaction system in which graphite, an intercalant and an oxidant are mixed. The mass ratio of graphite to oxidant is in the range of 0.1 to 1, and the mass ratio of graphite to intercalant is in the range of 0.01 to 0.
1. The oxidant includes potassium permanganate, and the intercalant includes concentrated phosphoric acid or concentrated sulfuric acid. The concentration of concentrated sulfuric acid is 70 to 98 wt%, and the concentration of concentrated phosphoric acid is ≥ 70 wt%. When diluted with water, the mass ratio of graphite to water ranges from 0.05 to 0.1; When the filter cake is washed with water, the washing frequency range is 1 to 5 times.
2. The method for cleaning graphite oxide without hydrochloric acid according to claim 1, characterized in that: The graphite includes one or a mixture of two or more of flake graphite, spherical graphite and expanded graphite. The flake graphite has a diameter range of 30 to 5000 mesh, the spherical graphite has a particle size range of 30 to 5000 mesh, and the expanded graphite has a particle size range of 30 to 5000 mesh.
3. The method for cleaning graphite oxide without hydrochloric acid according to claim 1, characterized in that: The solid-liquid separation and filter cake collection method includes one or a combination of two or more methods such as centrifugation, filter pressing and suction filtration.
4. The method for cleaning graphite oxide without hydrochloric acid according to claim 3, characterized in that: In the process of centrifugal collection of filter cake, the centrifugal speed is 1000 rpm~12000 rpm, and the centrifugal time is 10 min~30 min; in the process of collecting filter cake by pressure filtration, the filter cloth materials used include: polyethersulfone, nylon, polyester or polycarbonate, the pore size of the filter cloth is 100 mesh~5000 mesh, the filter plate and filter frame materials used include: stainless steel, polypropylene, polyethylene or polytetrafluoroethylene, the filtration equipment includes: bell-type filter press, plate and frame filter press, diaphragm filter press or hydraulic press, and the pressure range used is 0.1 MPa~20 MPa; in the process of collecting filter cake by suction filtration, the filter membrane materials used include: polyethersulfone, nylon, polyester, mixed cellulose or polycarbonate, and the pore size of the filter membrane is 0.1 μm~20 μm.
5. The method for cleaning graphite oxide without hydrochloric acid according to claim 1, characterized in that: When water and hydrogen peroxide are added to form slurry, the mass fraction of hydrogen peroxide in hydrogen peroxide ranges from 10% to 30%, the mass ratio of graphite to water ranges from 0.001 to 0.1, and the mass ratio of graphite to hydrogen peroxide ranges from 0.01 to 1.
6. The method for cleaning graphite oxide without hydrochloric acid according to claim 1, characterized in that: The high-purity graphite oxide filter cake has a solid mass fraction of 10-50% and an impurity mass fraction of less than 0.5%.