A method for preparing a catalyst for saturation of distillate oil aromatics
By adding specific additives to the active metal impregnating liquid of the distillate aromatic catalyst, an active stack is formed that is beneficial to aromatic adsorption, solving the problem of insufficient catalyst hydrogenation activity in the existing technology, achieving efficient aromatic saturation effect and reducing production costs.
Patent Information
- Application Number
- CN202111536353.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-12-14
AI Technical Summary
In the existing technology, the hydrogenation activity of distillate aromatic hydrocarbon saturated catalysts is insufficient. Especially when producing No. 3 jet fuel from low-smoke point kerosene, it is difficult to deeply remove monocyclic and bicyclic aromatic hydrocarbons, and precious metal catalysts are susceptible to sulfide poisoning, and non-noble metal catalysts are susceptible to sulfide poisoning. The catalyst preparation process is cumbersome and costly.
By adding active metal guiding aids such as nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid and diethylenetriaminepentaacetic acid into the active metal impregnating solution, the active metal is guided to form an active pile on the surface of the carrier that is conducive to the adsorption of aromatic hydrocarbon molecules. Stacking prolongs the residence time and reaction time of aromatic molecules on the catalyst, thereby improving the aromatic saturation activity of the catalyst.
The aromatic hydrocarbon saturation activity of the catalyst is significantly improved, the hydrogenation ability of monocyclic and bicyclic aromatic hydrocarbons is enhanced, the production cost is reduced, and the stability and economy of the catalyst are improved.
Smart Images

Figure BDA0003410136740000111 
Figure BDA0003410136740000112 
Figure BDA0003410136740000121
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a distillate oil aromatic saturation catalyst, in particular to a high-activity supported non-precious metal aromatic saturation catalyst and a preparation method thereof. Background Art
[0002] As the trend of crude oil becoming inferior and heavier accelerates, the aromatic content of crude oil continues to increase during the hydrorefining process of jet fuel and diesel. Aromatics in petroleum fractions mainly include the following four categories:
[0003] (1) Monocyclic aromatic hydrocarbons, including benzene, alkylbenzenes, benzocycloalkanes, etc.;
[0004] (2) Bicyclic aromatic hydrocarbons, including naphthalene and alkylnaphthalene, biphenyl and naphthocycloalkanes;
[0005] (3) tricyclic aromatic hydrocarbons, including anthracene, phenanthrene, fluorene and their alkyl derivatives;
[0006] (4) Polycyclic aromatic hydrocarbons, such as pyrene, fluoranthene, etc.
[0007] The aromatic nucleus in aromatic hydrocarbons is very stable and it is difficult to directly break and open the ring. The condensed rings and polycyclic rings of macromolecules can only open the rings and further undergo cracking reactions after the aromatic rings are hydrogenated and saturated. Studies have shown that the hydrogenation reaction of aromatic hydrocarbons has the following rules:
[0008] ① The equilibrium constant of aromatic hydrogenation reaction decreases with the increase of reaction temperature;
[0009] ② In the range of 600K to 700K, the equilibrium constant lgKp value of the complete hydrogenation saturation reaction of aromatics decreases as the number of rings in the molecule increases;
[0010] ③ In the range of 600K to 700K, the equilibrium constant of the first ring hydrogenation saturation reaction in condensed ring aromatics is the largest, and the equilibrium constants of the second and third ring saturation reactions decrease in turn;
[0011] ④ When the temperature exceeds 600K, the equilibrium constant of the aromatic hydrogenation saturation reaction is relatively small, so it is necessary to use a higher pressure to improve the equilibrium conversion rate;
[0012] ⑤ The hydrogenation saturation of the first aromatic ring in condensed aromatic hydrocarbons is relatively easy, and its relative reaction rate constant is 1.38, which is 10 times that of benzene hydrogenation. However, the hydrogenation saturation of the remaining aromatic rings is relatively difficult, and its reaction rate is close to that of benzene.
[0013] In industry, there are two main processes for aromatic saturation of distillate oil: one-stage process and two-stage process. The catalysts used are supported metal sulfide and supported precious metal catalysts. When the sulfur and nitrogen content in the crude oil is high, γ-Al is usually used. 2 O3 Supported sulfided NiMo, NiW, CoMo catalysts. When the sulfur and nitrogen content in the feed oil is low enough, the use of highly active supported precious metal catalysts is more effective.
[0014] The advantage of the one-stage process is that it is not affected by poisons in the raw materials to be treated; its disadvantage is that the hydrogenation activity is not high and the reaction rate is very slow under normal hydrogenation treatment conditions. To achieve a higher aromatic removal depth, harsh reaction conditions (360-425°C) are usually required, and at high temperatures, thermodynamic equilibrium limits the depth of aromatic hydrogenation.
[0015] The two-stage process is to carry out desulfurization and dearomatization in stages. The first stage uses a traditional sulfide catalyst to reduce the S content through harsh hydrogenation treatment, and the second stage uses a precious metal catalyst for aromatic saturation. Its advantages are that aromatics can be deeply removed and the reaction conditions are relatively mild (150-350°C); its disadvantage is that the second stage catalyst is very sensitive to sulfides in the raw materials, requiring the S content in the product to be reduced to ppm level after one stage of refining.
[0016] The aromatic content is directly related to the smoke point of jet fuel. The specification of No. 3 jet fuel requires that the volume content of aromatics should not exceed 20.0% and the smoke point should not be less than 25.0 mm. For straight-run kerosene fractions, it mainly contains single-ring and double-ring aromatics, and basically does not contain three-ring and above aromatics. The single-ring aromatics mainly include alkylbenzenes, indanes, tetralins, and indenes, and the double-ring aromatics mainly include naphthalene and naphthalenes. The difficulty of hydrogenation saturation of single-ring and double-ring aromatics is higher than that of multi-ring aromatics. Therefore, the development of catalysts with higher aromatic saturation activity is of great significance for the production of No. 3 jet fuel using low smoke point kerosene as raw material.
[0017] At present, there are three main types of aromatic saturation catalysts that are being studied more:
[0018] (1) Non-precious metal sulfide catalysts. The advantages of this type of catalyst are that it is not sensitive to the poisoning effect of sulfide species in the raw materials and has strong adaptability. It is also the most widely used in industry at present, but it generally has the problem of low hydrogenation activity;
[0019] (2) Precious metal catalysts: This type of catalyst has high hydrogenation activity and can achieve deep saturation of aromatics under relatively mild conditions. However, when the raw material contains a high amount of sulfides, it is very easy to cause catalyst poisoning and deactivation, and the production cost is high.
[0020] (3) Other types of catalysts, mainly including amorphous alloy catalysts, transition metal carbon or nitride catalysts, etc., but these catalysts have harsh preparation conditions, poor stability and high production costs, which limits their large-scale application.
[0021] Chinese patent CN101099934A discloses a metal nitride catalyst for saturated hydrogenation of aromatics, wherein nickel-molybdenum bimetallic nitride is loaded on alumina, stirred and impregnated at room temperature for 2-4 hours, filtered, fully dried, vacuum dried at 60-100°C for 5-8 hours, pressed into tablets, sieved, and directly heated and calcined. The process is as follows: in an Ar gas flow, the temperature is raised from room temperature to 650-680°C at a rate of 10°C / min, maintained for 2 hours, and the Ar gas space velocity is 500-1500h -1 ; Switch H 2 The airflow was maintained for 2 h, and then 2 Cool to room temperature, H 2 Airspeed: 500~1500h -1 Finally, in the presence of 1% O 2 N 2 The catalyst is passivated for 4 hours and used for saturated hydrogenation of monocyclic and bicyclic aromatic hydrocarbons with high catalytic activity. The defects of this technology or the shortcomings of the present invention are as follows: the calcination process of the catalyst prepared by this method is relatively complicated, the production cost is high, and it is not economical enough.
[0022] Chinese patent CN105521797B discloses a supported bimetallic component catalyst and a preparation method thereof, comprising impregnating a carrier with a compound containing a first active metal component and a compound containing a second active metal component, reducing and activating the carrier, and impregnating the reduced and activated product with a solution containing the second metal active component in a reducing or inert atmosphere, wherein the prepared catalyst has significantly higher aromatic saturation activity. The defects of this technology or the shortcomings of the present invention are: the catalyst prepared by this method requires the use of precious metals, and the economic cost is relatively high.
[0023] Chinese patent CN106582707B discloses a supported alloy type aromatic hydrocarbon saturation catalyst and its preparation method, which mainly solves the problem of low hydrogenation saturation of polycyclic aromatic hydrocarbons existing in the prior art. By using a catalyst selected from at least one of aluminum oxide, silicon oxide, titanium oxide or amorphous silicon aluminum as a carrier, and an alloy formed by precious metals and non-precious metals as an active component, it has the characteristics of high hydrogenation saturation activity. The defects of this technology or the shortcomings of the present invention are: the catalyst prepared by this method needs to use precious metals, and the economic cost is relatively high.
[0024] US Patent No. 5,308,814 discloses a variety of carrier materials for a noble metal dearomatization catalyst composition, wherein the carrier is prepared from Y and a high temperature resistant inorganic oxide (such as silicon dioxide, alumina, or silicon dioxide and alumina), and platinum and palladium are loaded, wherein the proportion of Y zeolite in the carrier is 10-90%. The defects of this technology or the shortcomings of the present invention are: the use of noble metals and molecular sieves has high production costs.
[0025] Therefore, it is necessary to provide a highly active catalyst for the saturation of distillate aromatics. Summary of the invention
[0026] The technical problem to be solved by the present invention is to develop a preparation method of a high-activity aromatic saturation catalyst for the aromatic saturation of distillate oil, especially suitable for producing No. 3 jet fuel with an aromatic content of not more than 20.0v% and a smoke point of not less than 25.0mm using straight-run kerosene as raw material.
[0027] In order to solve the above problems, the present invention provides a method for preparing a distillate oil aromatic saturation catalyst. The preparation method of the present invention adds an active metal guiding agent during the preparation of the active metal impregnation solution to guide the active metal to form active stacking on the carrier surface that is beneficial to the adsorption of aromatic molecules, selectively prolonging the residence time and reaction time of the aromatic molecules in the crude oil on the catalyst, thereby greatly improving the aromatic saturation activity of the catalyst.
[0028] The method for preparing the distillate oil aromatic saturation catalyst of the present invention comprises the following steps:
[0029] (1) Pseudo-boehmite powder and Tianqing powder are uniformly mixed, and then a peptizing agent and deionized water are added to mix and knead, and then extruded, dried, and calcined to obtain a carrier;
[0030] (2) preparing an active metal impregnation solution, and adding active metal directing aids such as nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid and diethylenetriaminepentaacetic acid during the preparation process;
[0031] (3) The carrier of step (1) is impregnated with the active metal impregnation solution of step (2), dried and calcined in an oxygen-containing atmosphere to obtain a distillate oil aromatic saturation catalyst.
[0032] The method for preparing a distillate oil aromatic saturation catalyst of the present invention comprises the following steps: in step (1), the ratio of the pseudo-boehmite powder, the field pine powder, the peptizing agent and the deionized water is (100-300): (5-20): (4-18): (80-260).
[0033] The preparation method of the fraction oil aromatic saturation catalyst of the present invention comprises the following peptizing agents: citric acid and nitric acid.
[0034] In the method for preparing the distillate oil aromatic saturation catalyst of the present invention, the active metal is at least one of Co, Mo, Ni and W.
[0035] The method for preparing a distillate oil aromatic saturation catalyst of the present invention, in step (2), the mass ratio of nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid, diethylenetriaminepentaacetic acid and active metals Mo, Ni, W, Co is (10-35): (13-42): (28-65): (8-47): (150-1200): (50-500): (200-1800): (50-500).
[0036] The method for preparing a distillate oil aromatic saturation catalyst of the present invention comprises the following mass ratios: (14-33) of nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid, diethylenetriaminepentaacetic acid and active metal: (16-37) : (31-59) : (11-43) : (200-1000) : (80-300) : (400-1500) : (80-300) .
[0037] The preparation method of the distillate oil aromatic saturation catalyst of the present invention comprises the following steps: in step (3), the drying temperature is 50°C to 150°C, the time is 2h to 40h, and the calcination temperature is 300°C to 600°C, the time is 2h to 20h.
[0038] The preparation method of the distillate oil aromatic saturation catalyst of the present invention comprises the following steps: the drying temperature is 50-120°C, the time is 2-20 hours, and the calcination temperature is 300-500°C, the time is 2-10 hours.
[0039] The preparation method of the distillate oil aromatic saturation catalyst of the present invention comprises the following steps: in step (1), the drying temperature is 50°C to 150°C, and the time is 2h to 40h; the calcination temperature is 300°C to 800°C, and the time is 2h to 20h.
[0040] The preparation method of the distillate oil aromatic saturation catalyst of the present invention, the carrier is γ-Al 2 O 3 Support or γ-Al modified with Ti, Mg, B, P additives 2 O 3 Carrier; the Ti, Mg, B, P additives are added during the production process of pseudo-boehmite, or are added during the extrusion process.
[0041] The present invention can also be described in detail as follows:
[0042] A method for preparing a supported non-precious metal hydrogenation catalyst with high aromatic saturation activity comprises the following steps:
[0043] (1) Pseudo-boehmite powder and a certain proportion of Tianqing powder are mixed evenly, and then a peptizing agent, deionized water, etc. are added to mix and knead, and then extruded, dried, and roasted to obtain γ-Al 2 O 3Support or γ-Al modified with additives such as Ti, Mg, B, P, etc. 2 O 3 carrier.
[0044] (2) An active metal impregnation solution is prepared by using one or more compounds containing Co, Mo, Ni, and W. When preparing the impregnation solution, nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid, diethylenetriaminepentaacetic acid and other substances are added in a certain proportion to form a precursor with the active metal species. The preferred mass ratio of nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid, and diethylenetriaminepentaacetic acid is (10-35): (13-42): (28-65): (8-47). Nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid, diethylenetriaminepentaacetic acid and other substances are used to form a precursor with the active metal species, so that when the active metal is loaded on the surface of the carrier, an active stacking that is conducive to the adsorption of aromatic molecules is formed, and the residence time and reaction time of aromatic molecules in the crude oil on the catalyst are selectively extended, thereby greatly improving the aromatic saturation activity of the catalyst. The more preferred mass ratio of the four species of nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid and diethylenetriaminepentaacetic acid is (14-33): (16-37): (31-59): (11-43).
[0045] (3) The carrier obtained in step (1) is impregnated with the impregnation solution of step (2), dried and calcined in an oxygen-containing atmosphere to obtain a finished catalyst. The drying process is carried out at 50°C to 150°C for 2h to 40h. The calcination process is carried out at 300°C to 600°C for 2h to 20h. More preferably, the drying process is carried out at 50°C to 120°C for 2h to 20h, and the calcination process is carried out at 300°C to 500°C for 2h to 10h.
[0046] The invention discloses a preparation method of a catalyst for the saturation of aromatic hydrocarbons in distillate oil, wherein the active metal component of the catalyst contains one or more of Co, Mo, Ni and W. In the preparation process of the catalyst, by adding nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid, diethylenetriaminepentaacetic acid and other substances in a certain proportion to an impregnation liquid, the active metal is guided to form active stacking on the surface of a carrier that is conducive to the adsorption of aromatic hydrocarbon molecules, and the residence time and reaction time of aromatic hydrocarbon molecules in the raw oil on the catalyst are selectively prolonged, thereby greatly improving the aromatic hydrocarbon saturation activity of the catalyst.
[0047] A certain proportion of nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid, diethylenetriaminepentaacetic acid and other substances can form complexes with active metal ions such as Co, Mo, Ni, and W in a certain proportion in the solution. The formation of the complex has a great influence on the structure of the active metal species, causing the number of stacking layers and edge length to change. At a certain concentration, an active phase with a high stacking state and a small sheet length can be generated, providing a more suitable physical and chemical environment for the aromatic hydrocarbon saturation reaction. On the other hand, the formation of the complex has a sticky and anchoring effect on the active metal, preventing it from aggregating and migrating on the surface during the drying and roasting process to form overly large particles of metal, thereby improving the utilization efficiency of the active metal.
[0048] The catalyst prepared by the present invention is characterized in that an active metal guiding aid is added to the impregnation solution to guide the active metal to be loaded on the carrier surface in the form of a stack, thereby forming an active stack with a specific morphology, prolonging the residence time and reaction time of aromatic molecules in the crude oil, and promoting the conversion of aromatic molecules to cycloalkane molecules, thereby achieving the purpose of aromatic saturation. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 This is a transmission electron microscope photo of the catalyst in Example 1.
[0050] Figure 2 This is a transmission electron microscope photo of the catalyst in Example 2.
[0051] Figure 3 This is a transmission electron microscope photo of the catalyst in Example 3.
[0052] Figure 4 This is a transmission electron microscope photograph of the catalyst of Comparative Example 1.
[0053] Figure 5 This is a transmission electron microscope photograph of the catalyst of Comparative Example 2.
[0054] Figure 6 This is a transmission electron microscope photograph of the catalyst of Comparative Example 3. DETAILED DESCRIPTION
[0055] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.
[0056] Embodiment 1:
[0057] (1) γ-Al 2 O 3 Preparation of vector
[0058] Weigh 1000g of pseudo-boehmite powder, 55g of Tianqing powder, 25g of citric acid, and 650mL of 3-5% dilute nitric acid, mix them evenly, extrude them into strips using an extruder, dry them at 110℃ for 10h, and calcine them at 520℃ in air atmosphere to obtain γ-Al 2 O 3 carrier.
[0059] (2) Preparation of Mo-Ni impregnation solution containing active metal guiding additives
[0060] Weigh 500g of deionized water, add 8.5g of concentrated phosphoric acid, heat to 75°C while stirring, add 185g of molybdenum trioxide and 68g of basic nickel carbonate. After the solution is completely dissolved and transparent, add 3.3g of nitrilotriacetic acid, 4.7g of cyclohexanediaminetetraacetic acid, 10.4g of citric acid, and 5.2g of diethylenetriaminepentaacetic acid, heat to 90°C, and continue to maintain the temperature for 4h. After the constant temperature is completed, cool naturally to room temperature, dilute to 700mL with deionized water, and set aside.
[0061] (3) Mo-Ni / γ-Al 2 O 3 Catalyst preparation
[0062] Weigh 500 g of the carrier prepared in step (1), measure 350 mL of the impregnation solution prepared in step (2), impregnate equal volumes for 60 minutes, dry at 110° C. for 4 hours, and calcine at 480° C. for 8 hours to obtain a finished catalyst.
[0063] Embodiment 2:
[0064] (1) γ-Al containing Ti 2 O 3 Preparation of vector
[0065] Weigh 950g of pseudo-boehmite powder, 50g of metatitanic acid, 55g of Tianqing powder, 25g of citric acid, and 660mL of 3-5% dilute nitric acid, mix them evenly, extrude them into a strip using an extruder, dry them at 120℃ for 10h, and calcine them at 520℃ in air atmosphere to obtain Ti-containing γ-Al 2 O 3 carrier.
[0066] (2) Preparation of W-Ni impregnation solution containing active metal guiding additives
[0067] Weigh 500g of deionized water, add 247g of ammonium metatungstate and 178g of nickel nitrate while stirring. After the solution is completely dissolved and transparent, heat it to 95°C, add 7.8g of nitrilotriacetic acid, 5.9g of cyclohexanediaminetetraacetic acid, 7.3g of citric acid, and 2.6g of diethylenetriaminepentaacetic acid, and continue to maintain the constant temperature for 7.5h. After the constant temperature is completed, cool it naturally to room temperature, adjust the volume to 700mL, and set aside.
[0068] (3)W-Ni / γ-Al 2 O 3 Catalyst preparation
[0069] Weigh 500 g of the carrier prepared in step (1), measure 360 mL of the impregnation solution prepared in step (2), impregnate for 55 minutes with equal volumes, dry at 105° C. for 4 hours, and calcine at 500° C. for 6 hours to obtain a finished catalyst.
[0070] Embodiment 3:
[0071] (1) Boron-containing γ-Al 2 O 3 Preparation of vector
[0072] Weigh 1000g boron-modified pseudo-boehmite powder, 50g Tianqing powder, 13g citric acid, and 640mL of 3-5% dilute nitric acid, mix them evenly, extrude them into a strip using an extruder, dry them at 120℃ for 10h, and calcine them at 520℃ in air atmosphere to obtain B-containing γ-Al 2 O 3 carrier.
[0073] (2) Preparation of W-Mo-Ni impregnation solution containing active metal guiding additives
[0074] Weigh 500g of deionized water, add 22g of phosphoric acid while stirring, heat to 80℃, add 65g of molybdenum trioxide and 78g of nickel nitrate, wait until they are completely dissolved and the solution is transparent, cool to 40℃, add 167g of ammonium metatungstate and completely dissolve. Heat to 95℃, add 3.3g of nitrilotriacetic acid, 4.0g of cyclohexanediaminetetraacetic acid, 11.6g of citric acid, and 4.7g of diethylenetriaminepentaacetic acid, and continue to maintain constant temperature for 9h. After the constant temperature is over, cool naturally to room temperature, dilute to 700mL, and set aside.
[0075] (3)W-Mo-Ni / γ-Al 2 O 3 Catalyst preparation
[0076] Weigh 500 g of the carrier prepared in step (1), measure 355 mL of the impregnation solution prepared in step (2), impregnate equal volumes for 75 minutes, dry at 115° C. for 4 hours, and calcine at 500° C. for 5 hours to obtain a finished catalyst.
[0077] Embodiment 4:
[0078] (1) γ-Al containing Mg 2 O 3 Preparation of vector
[0079] Weigh 1000g of Mg-modified pseudo-boehmite powder, 50g of Tianqing powder, 13g of citric acid, and 640mL of 3-5% dilute nitric acid, mix them evenly, extrude them into a strip using an extruder, dry them at 120℃ for 10h, and calcine them at 520℃ in air atmosphere to obtain Mg-containing γ-Al 2 O 3 carrier.
[0080] (2) Preparation of Mo-Co impregnation solution containing active metal directing additives
[0081] Weigh 500g of deionized water, add 24g of phosphoric acid while stirring, heat to 80°C, add 215g of molybdenum trioxide and 78g of cobalt nitrate, heat to 95°C, wait until completely dissolved, add 3.3g of nitrilotriacetic acid, 4.0g of cyclohexanediaminetetraacetic acid, 11.6g of citric acid, and 4.7g of diethylenetriaminepentaacetic acid, and continue to keep the temperature constant for 9h. After the solution becomes transparent, cool to 40°C. After the constant temperature is over, cool naturally to room temperature, dilute to 700mL, and set aside.
[0082] (3) Mo-Co / γ-Al 2 O 3 Catalyst preparation
[0083] Weigh 500 g of the carrier prepared in step (1), measure 355 mL of the impregnation solution prepared in step (2), impregnate equal volumes for 75 minutes, dry at 115° C. for 4 hours, and calcine at 500° C. for 5 hours to obtain a finished catalyst.
[0084] Embodiment 5:
[0085] (1) γ-Al containing P 2 O 3 Preparation of vector
[0086] Weigh 1000g P-modified pseudo-boehmite powder, 52g Tianqing powder, 14g citric acid, and 630mL of 3-5% dilute nitric acid, mix them evenly, extrude them into a strip, dry them at 120℃ for 10h, and calcine them at 520℃ in air atmosphere to obtain P-containing γ-Al 2 O 3 carrier.
[0087] (2) Preparation of Mo-Co impregnation solution containing active metal directing additives
[0088] Weigh 500g of deionized water, add 24g of phosphoric acid while stirring, heat to 80°C, add 215g of molybdenum trioxide and 78g of cobalt nitrate, heat to 95°C, wait until completely dissolved, add 3.5g of nitrilotriacetic acid, 1.3g of cyclohexanediaminetetraacetic acid, 2.8g of citric acid, and 2.4g of diethylenetriaminepentaacetic acid, and continue to keep the temperature constant for 9h. After the solution becomes transparent, cool to 40°C. After the constant temperature is over, cool naturally to room temperature, dilute to 700mL, and set aside.
[0089] (3) Mo-Co / γ-Al 2 O 3 Catalyst preparation
[0090] Weigh 500 g of the carrier prepared in step (1), measure 355 mL of the impregnation solution prepared in step (2), impregnate equal volumes for 75 minutes, dry at 115° C. for 4 hours, and calcine at 500° C. for 5 hours to obtain a finished catalyst.
[0091] Comparative Example 1:
[0092] (1) γ-Al 2 O 3 Preparation of vector
[0093] Weigh 1000g of pseudo-boehmite powder, 55g of Tianqing powder, 25g of citric acid, and 650mL of 3-5% dilute nitric acid, mix them evenly, extrude them into strips using an extruder, dry them at 110℃ for 10h, and calcine them at 520℃ in air atmosphere to obtain γ-Al 2 O 3 carrier.
[0094] (2) Preparation of impregnation solution containing active metal Mo-Ni
[0095] Weigh 500g of deionized water, add 8.5g of concentrated phosphoric acid, heat to 75°C while stirring, add 185g of molybdenum trioxide and 68g of basic nickel carbonate, wait until they are completely dissolved and the solution is transparent, cool naturally to room temperature, and dilute to 700mL for later use.
[0096] (3) Mo-Ni / γ-Al 2 O 3 Catalyst preparation
[0097] Weigh 500 g of the carrier prepared in step (1), measure 350 mL of the impregnation solution prepared in step (2), impregnate equal volumes for 60 minutes, dry at 110° C. for 4 hours, and calcine at 480° C. for 8 hours to obtain a finished catalyst.
[0098] Comparative Example 2:
[0099] (1) γ-Al containing Ti 2 O 3Preparation of vector
[0100] Weigh 950g of pseudo-boehmite powder, 50g of metatitanic acid, 55g of Tianqing powder, 25g of citric acid, and 660mL of 3-5% dilute nitric acid, mix them evenly, extrude them into a strip using an extruder, dry them at 120℃ for 10h, and calcine them at 520℃ in air atmosphere to obtain Ti-containing γ-Al 2 O 3 carrier.
[0101] (2) Preparation of impregnation solution containing active metal W-Ni
[0102] Weigh 500g of deionized water, add 247g of ammonium metatungstate and 178g of nickel nitrate into it while stirring. After they are completely dissolved and the solution becomes transparent, dilute to 700mL and set aside.
[0103] (3)W-Ni / γ-Al 2 O 3 Catalyst preparation
[0104] Weigh 500 g of the carrier prepared in step (1), measure 360 mL of the impregnation solution prepared in step (2), impregnate for 55 minutes with equal volumes, dry at 105° C. for 4 hours, and calcine at 500° C. for 6 hours to obtain a finished catalyst.
[0105] Comparative Example 3:
[0106] (1) Boron-containing γ-Al 2 O 3 Preparation of vector
[0107] Weigh 1000g boron-modified pseudo-boehmite powder, 50g Tianqing powder, 13g citric acid, and 640mL of 3-5% dilute nitric acid, mix them evenly, extrude them into a strip using an extruder, dry them at 120℃ for 10h, and calcine them at 520℃ in air atmosphere to obtain B-containing γ-Al 2 O 3 carrier.
[0108] (2) Preparation of W-Mo-Ni impregnation solution containing active metals
[0109] Weigh 500g of deionized water, add 22g of phosphoric acid thereto while stirring, heat to 80°C, add 65g of molybdenum trioxide and 78g of nickel nitrate, wait until they are completely dissolved and the solution becomes transparent, cool to 40°C, add 167g of ammonium metatungstate and completely dissolve, cool naturally to room temperature, and dilute to 700mL for use.
[0110] (3)W-Mo-Ni / γ-Al 2 O 3 Catalyst preparation
[0111] Weigh 500 g of the carrier prepared in step (1), measure 355 mL of the impregnation solution prepared in step (2), impregnate equal volumes for 75 minutes, dry at 115° C. for 4 hours, and calcine at 500° C. for 5 hours to obtain a finished catalyst.
[0112] Example 1 and Comparative Example 1, Example 2 and Comparative Example 2, Example 3 and Comparative Example 3 correspond to each other, and active metal directing aids are added in a certain proportion in the examples, while no active metal directing aids are added in the comparative examples.
[0113] The transmission electron microscope photos of the catalysts prepared in Examples 1 to 3 and Comparative Examples 1 to 3 are as follows: Figure 1 to Figure 6 As can be seen from the figure, the catalyst surface prepared according to the method of the present invention has an obvious stacking structure, while the active metal on the catalyst surface prepared by the conventional method is uniformly dispersed and no such structure is found.
[0114] The catalysts prepared in the above examples and comparative examples were subjected to 200 mL scale hydrogenation activity evaluation, and the evaluation feedstock oil was low-quality kerosene from a petrochemical company. The properties of the feedstock oil and the evaluation results of the examples are shown in Table 1, and the evaluation results of the comparative examples are shown in Table 2. As can be seen from Table 1 and Table 2, compared with the three comparative examples, the hydrogenation activity of the catalysts in the examples is significantly improved, the aromatic saturation ratio and the smoke point are increased to a greater extent, and the desulfurization and denitrification rates are also higher.
[0115] Table 1 Catalyst activity evaluation results of the examples
[0116]
[0117] Table 2 Comparative Example Catalyst Activity Evaluation Results
[0118]
[0119]
[0120] Note: (1) Sulfidation conditions: The catalyst was first pre-sulfurized at 330°C in a hydrogen atmosphere with kerosene containing 2ω% carbon disulfide at a pressure of 7.0 MPa for 20 h, and then the raw materials were added;
[0121] (2) Reaction conditions: reaction temperature 330°C, pressure 6.0 MPa, space velocity (volume) 1.5 h -1 , hydrogen to oil (volume) ratio is 400.
Claims
1. A method for preparing a distillate oil aromatic saturation catalyst, characterized in that: The following steps are involved: (1) Pseudo-boehmite powder and sesbania powder are uniformly mixed, and then a peptizing agent and deionized water are added to mix and knead, and then extruded, dried, and calcined to obtain a γ-Al2O3 carrier; (2) preparing an active metal impregnation solution, and adding active metal directing agents such as nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid and diethylenetriaminepentaacetic acid during the preparation process; (3) impregnating the support of step (1) into the active metal impregnation solution of step (2), drying and calcining in an oxygen-containing atmosphere to obtain a distillate oil aromatic saturation catalyst; The active metal is at least one of Co, Mo, Ni and W; In step (2), the mass ratio of nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid, diethylenetriaminepentaacetic acid and active metals Mo, Ni, W and Co is (10-35): (13-42): (28-65): (8-47): (150-1200): (50-500): (200-1800): (50-500).
2. The method for preparing a distillate oil aromatic saturation catalyst according to claim 1, characterized in that: In step (1), the ratio of the pseudo-boehmite powder, sesbania powder, peptizing agent and deionized water is (100-300): (5-20): (4-18): (80-260).
3. The method for preparing a distillate oil aromatic saturation catalyst according to claim 1, characterized in that: The peptizing agents are citric acid and nitric acid.
4. The method for preparing a distillate oil aromatic saturation catalyst according to claim 1, characterized in that: The mass ratio of the nitrilotriacetic acid, cyclohexanediaminetetraacetic acid, citric acid, diethylenetriaminepentaacetic acid and the active metals Mo, Ni, W and Co is (14-33): (16-37): (31-59): (11-43): (200-1000): (80-300): (400-1500): (80-300).
5. The method for preparing a distillate oil aromatic saturation catalyst according to claim 1, characterized in that: In step (3), the drying temperature is 50°C to 150°C, and the time is 2h to 40h; the calcination temperature is 300°C to 600°C, and the time is 2h to 20h.
6. The method for preparing a distillate oil aromatic saturation catalyst according to claim 5, characterized in that: The drying temperature is 50° C. to 120° C., and the time is 2 h to 20 h. The calcination temperature is 300° C. to 500° C., and the time is 2 h to 10 h.
7. The method for preparing a distillate oil aromatic saturation catalyst according to claim 1, characterized in that: In step (1), the drying temperature is 50°C to 150°C, and the time is 2h to 40h; the calcination temperature is 300°C to 800°C, and the time is 2h to 20h.
8. The method for preparing a distillate oil aromatic saturation catalyst according to claim 1, characterized in that: The carrier is a γ-Al2O3 carrier modified with Ti, Mg, B and P additives; the Ti, Mg, B and P additives are added during the production process of pseudo-boehmite or during the extrusion process.