A method for pretreating the surface of high-voltage anode aluminum foil with corrosion holes

Through a two-step combination of pretreatment method, including acid solution polishing and doping corrosion inhibitor polymer film, the uniformity and pore convergence problems of corrosive pores on the surface of high-voltage anode aluminum foil are solved, and better capacitance performance is achieved.

CN116313529BActive Publication Date: 2024-11-15UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211500975.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-28
Publication Date
2024-11-15
Estimated Expiration
2042-11-28

AI Technical Summary

Technical Problem

The existing high-pressure anode aluminum foil surface pretreatment method is complicated in technology, and it is difficult to control the uniformity and pore convergence of corroded pores, and it is not effective to eliminate the impact of surface rolling and oxide film on pores.

Method used

Two-step combined pretreatment method is adopted: first polishing treatment is performed in an acid solution to remove surface crumbs and oxide films, and then a polymer film doped with corrosion inhibitor is assembled on the surface of the flattened aluminum foil to uniformize the resistance of the aluminum foil surface. and current distribution.

Benefits of technology

By removing surface rolling marks and oxide films, the flattening of the aluminum foil surface and the uniformity of current distribution are achieved, the phenomenon of hole convergence is reduced, and the specific capacitance and comprehensive performance of the high-voltage anode aluminum foil are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116313529B_ABST
    Figure CN116313529B_ABST
Patent Text Reader

Abstract

The invention discloses a method for pretreating the surface of high-voltage anode aluminum foil for corrosion pores, and relates to the field of manufacturing high-voltage anode aluminum foil used in high-performance aluminum electrolytic capacitors. The invention aims at the problems of uneven corrosion pores, tunnel hole merging, etc. in the manufacturing process of high-voltage anode aluminum foil. Before the corrosion pore process, the invention firstly uses an acid solution polishing to remove the rolling mark defects and oxide film on the surface of the aluminum foil, and further self-assembles a polymer film doped with a corrosion inhibitor on the surface of the aluminum foil after polishing and leveling. Through the two-step combined pretreatment, the uniformity of the corrosion pores of the aluminum foil is improved, and the merging phenomenon in the corrosion pores and hole expansion process is reduced, thereby improving the specific capacitance and comprehensive performance of the high-voltage anode aluminum foil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of manufacturing high-voltage anode aluminum foil for aluminum electrolytic capacitors, in particular to a method for pretreating the surface of high-voltage anode aluminum foil with corrosion holes. Background Art

[0002] As an important part of the electronic system, aluminum electrolytic capacitors are widely used in electronic circuits and have become one of the irreplaceable electronic components. With the continuous reduction in the size of electronic systems and the development of high-density assembly, aluminum electrolytic capacitors, as basic components, are required to have the characteristics of high capacity and miniaturization to meet the development needs of electronic products. At present, the anode aluminum foil for aluminum electrolytic capacitors is generally electrochemically corroded to generate a large number of tunnel holes on the surface of the anode aluminum foil to expand its surface area, that is, to increase the specific capacitance of the capacitor, so as to achieve the purpose of high capacity and miniaturization of the capacitor.

[0003] During the processing of electrolytic capacitor aluminum foil, in order to achieve a high cubic texture of aluminum foil, the surface of the aluminum foil needs to be rolled, which will inevitably lead to many rolling marks on the surface of the aluminum foil. In addition, defects will also be formed on the aluminum surface due to environmental, operational, equipment and other reasons. At the same time, a dense aluminum oxide film will be generated on the surface of the aluminum foil during the subsequent texture heat treatment. The presence of surface rolling marks, defects and aluminum oxide film causes the pore size and pore distribution of aluminum foil corrosion to be extremely uneven, which is an important reason for limiting the improvement of the specific capacitance of aluminum electrolytic capacitors. Therefore, if the surface pretreatment technology can effectively eliminate or reduce the side effects of surface rolling marks, defects and the dense oxide film generated by heat treatment on pores, the formation of criss-cross corrosion grooves on the surface of the aluminum foil during the corrosion pore process can be avoided. This is the key technology for achieving uniform pores in electrolytic capacitor aluminum foil. On the other hand, after eliminating or reducing surface rolling marks and oxide film pretreatment, if a polymer film doped with corrosion inhibitor is further assembled on the flattened surface of the aluminum foil, the uneven distribution of surface corrosion activity can be reduced, making the surface resistance of the aluminum foil consistent and the current distribution on the surface of the aluminum foil more uniform, thereby reducing the pore-joining phenomenon during corrosion pore formation and pore expansion, and further improving the specific capacitance and comprehensive performance of the high-voltage anode aluminum foil.

[0004] A Chinese patent with publication number 202210249621.8 discloses a method for mechanical pre-lithiation of medium- and high-voltage anode aluminum foil for aluminum electrolytic capacitors. This method uses mechanical pre-lithiation to emboss pits with lithium crystal nuclei on the surface of the aluminum foil to improve the uniformity of pore formation. Although this method improves the uniformity of tunnel holes generated on the surface during electrolytic corrosion pore formation of the aluminum foil, it only makes the corrosion pores inside the pits more uniform, and the problem of uneven corrosion pore formation in areas outside the pits still exists. A Chinese patent with publication number 202110658748.0 discloses a method for inducing uniform corrosion pore formation of medium- and high-voltage anode aluminum foil using nano-pits after anodization. This method uses anodization to generate an ordered porous aluminum oxide film on the surface of the aluminum foil, and then dissolves the aluminum oxide film and exposes the orderly distributed nano-pits on the aluminum foil substrate. The pits are used to regulate the nucleation position of the tunnel holes during the corrosion pore formation of the aluminum foil, thereby improving the distribution uniformity of the generated tunnel holes. The porous aluminum oxide film generated on the surface of the aluminum foil by this method has an obvious tendency to be distributed along the rolling marks, which causes the location of the subsequent corrosion pores to be distributed along the rolling marks. In addition, this method increases the complexity and cost of the process through the anodic oxidation method. The Chinese patent with publication number 201410599417.4 discloses a method for chemically depositing dispersed tin and zinc crystal nuclei on the surface of high-purity aluminum foil for medium and high voltage anodes, striving to induce corrosion pores by dispersing active metal crystal nuclei. However, it is difficult to control the position of the nucleus nucleation by directly dispersing tin and zinc crystal nuclei on the surface of the aluminum foil, and the uniformity of the dispersed crystal nuclei themselves is also difficult to control. The existing surface pretreatment method for corrosion pores of high-voltage anode aluminum foil mainly improves the uniformity of pores by introducing active sites or templates that induce corrosion pores in the surface pretreatment. However, these methods all have problems such as complex process flow, difficult control of active sites, and are not conducive to industrialization. Moreover, the current surface pretreatment technology only modifies the surface of the aluminum foil, and does not focus on eliminating the influence of surface rolling marks and oxide films on corrosion pores, nor does it propose targeted solutions to this problem. Therefore, since the distribution of active sites of corrosion pores on the surface of aluminum foil is difficult to be effectively controlled by pretreatment, the opposite is done, and the factors that cause uneven corrosion pore activity on the surface are removed to obtain a uniform surface state, so that the pores can be randomly distributed, and problems such as concentrated pores and pores can be avoided. Based on this idea, if the influence of the rolling mark defects and the oxide film on the surface of the aluminum foil can be eliminated first, a relatively smooth aluminum foil surface can be obtained, and then the surface activity unevenness can be eliminated by an effective surface self-assembled film layer, the corrosion pores can be randomly and evenly distributed, thereby obtaining a better surface modification effect. To this end, the present invention is proposed to achieve the above purpose. Summary of the invention

[0005] The present invention aims to provide a method for pretreating the surface of corrosion pores of high-voltage anode aluminum foil, and relates to the high-voltage anode aluminum foil used in the manufacture of high-performance aluminum electrolytic capacitors. Aiming at the problem that the rolling mark defects and oxide film on the surface of the aluminum foil affect the uniformity of corrosion pores and the serious pore merging, the present invention adopts a technical idea of ​​eliminating the uneven state of surface activity by a two-step combined pretreatment, firstly eliminating the surface rolling mark defects and oxide film by polishing with an acid pickling solution to obtain a flat aluminum foil surface, and further assembling a polymer film doped with a corrosion inhibitor on the flattened aluminum foil surface to eliminate the uneven state of corrosion pore activity, so that the surface resistance of the aluminum foil is consistent, and the current distribution on the surface of the aluminum foil is more uniform, thereby reducing the pore merging phenomenon in the process of corrosion pores and pore expansion, and further improving the specific capacitance and comprehensive performance of the high-voltage anode aluminum foil.

[0006] A method for pretreating the surface of a high-voltage anode aluminum foil with corrosion holes, using a two-step combined pretreatment method to perform surface treatment on the high-voltage anode aluminum foil, the specific steps are as follows:

[0007] Step 1: polishing the surface of the high voltage anode aluminum foil in an acid solution;

[0008] Step 2: Assemble an organic polymer film doped with a corrosion inhibitor on the polished aluminum foil surface.

[0009] Furthermore, the surface polishing described in step 1 is to immerse the aluminum foil in an acidic solution for chemical polishing, the acidic solution is a 0.1-1.5 mol / L HNO3 solution, the polishing solution temperature is 25-80°C, and the treatment time is 0.5-10 min.

[0010] Furthermore, the implementation method of the surface assembly of the organic polymer film doped with the corrosion inhibitor in step 2 is to mix the corrosion inhibitor with the organic polymer to prepare an aqueous solution, and then immerse the aluminum foil in the aqueous solution to perform surface self-assembly to form the film.

[0011] Furthermore, the corrosion inhibitor in step 2 is cerium salt, molybdate, tungstate, vanadate, borate, phosphate, or silicate. The corrosion inhibitor can be one of the salts or a mixture of any two or more salts.

[0012] Furthermore, the organic polymer described in step 2 is one or a combination of silane, polyethylene glycol, polyaniline, imidazoline acrylate, imidazoline oleate, 8-hydroxyquinoline, benzotriazole, and oleic acid.

[0013] Furthermore, the concentration of the corrosion inhibitor in step 2 is 0.1-2.0 mmol / L, and the concentration of the organic polymer in the aqueous solution is 0.1-5 wt.%.

[0014] Furthermore, the temperature of the surface self-assembly solution is 25-80° C., and the soaking time is 0.5-15 min.

[0015] Beneficial effects of the present invention:

[0016] (1) The surface of the high-voltage anode aluminum foil is polished in an acidic solution. The acidic solution can dissolve the surface oxide film of the aluminum foil and the protruding aluminum matrix at the rolling mark. The surface rolling marks, defects and oxide film formed on the surface of the high-voltage aluminum foil during the production process can be effectively removed, making the surface of the aluminum foil smooth, reducing tip discharge and defect aggregation, and facilitating the uniform distribution of pitting initiation in the subsequent electrochemical corrosion process.

[0017] (2) The surface of the aluminum foil after surface polishing and leveling is further assembled with an organic polymer film doped with a corrosion inhibitor. By utilizing the corrosion inhibition effect of the corrosion inhibitor and the shielding and blocking synergistic effect of the organic polymer film, the uneven corrosion activity on the surface of the aluminum foil is further eliminated. The formed organic polymer film doped with a corrosion inhibitor can effectively increase the uniformity of the surface resistance of the aluminum foil. During the electrochemical pore formation process, the current distribution on the surface of the aluminum foil is made more uniform, further improving the uniformity of corrosion pore formation.

[0018] (3) Through the above two-step combined pretreatment of the surface of the high-voltage anode aluminum foil, the uniformity and surface density of the corrosion pores in the aluminum foil can be improved, the pore-forming phenomenon can be reduced, and the specific capacitance of the aluminum foil can be increased, thereby improving the performance of the aluminum electrolytic capacitor. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The surface morphology (a) and the pore size distribution diagram (b) of the perforated foil without surface pretreatment of comparative example 1 are shown;

[0020] Figure 2 The surface morphology (a) and the pore size distribution diagram (b) of the porous foil after chemical deposition of tin crystal nuclei on the surface of comparative example 2;

[0021] Figure 3a This is a surface morphology of the porous foil after acid solution polishing and assembly of the corrosion inhibitor-doped organic polymer film pretreatment in Example 5;

[0022] Figure 3b This is the distribution diagram of the tunnel pore size on the surface of the porous foil in Example 5 after being polished with an acid solution and pretreated with an organic polymer film doped with a corrosion inhibitor. DETAILED DESCRIPTION

[0023] The above method is further described below in conjunction with embodiments, but does not constitute any limitation to the present invention. Any limited modifications made within the scope of protection of the claims of the present invention are still within the scope of protection of the claims of the present invention.

[0024] Comparative Example 1

[0025] A pore-forming solution with a concentration of 3.5 mol / L H2SO4+0.7 mol / L HCl was prepared and heated to 70°C. A 120 μm thick electrolytic capacitor high-voltage anode aluminum foil (without surface pretreatment) containing trace amounts of Cu, Si, and Fe elements and with a purity of 99.99 wt.%, a {100} texture occupancy of more than 97%, and a direct current was applied therein to perform corrosion pore-forming. The corrosion pore-forming time was 80 s and the pore-forming current density was 250 mA / cm 2 , the pore charge density is 20C / cm 2 The aluminum foil without surface pretreatment was corroded and pores were formed by scanning electron microscope. The pore size distribution of the surface tunnel holes was statistically analyzed. Figure 1 .

[0026] Comparative Example 2

[0027] China Patent Publication No. 201410599417.4 discloses a method for chemically depositing dispersed tin and zinc crystal nuclei on the surface of high-purity aluminum foil for medium and high voltage anodes. A high-voltage anode aluminum foil with an Al purity of 99.99%, a thickness of 110μm, and a {100} surface texture occupancy rate of more than 95% is placed in a 90°C 15mol / L phosphoric acid + 5mol / L sulfuric acid mixed solution for 50 seconds to form a new water-containing film on the surface of the aluminum foil. The above aluminum foil is placed in a solution for chemical deposition of tin crystal nuclei. The solution composition is: 0.2mol / L sodium stannate + 0.1mol / L sodium hydroxide + 0.005mol / L potassium sodium tartrate; the chemical deposition temperature is 50°C, and the chemical deposition time is 20 seconds.

[0028] The aluminum foil with dispersed tin crystal nuclei obtained by chemical deposition on the surface was subjected to pore etching. The pore etching solution was 3.5 mol / L H2SO4 + 0.7 mol / L HCl aqueous solution. The temperature was 70°C. The pore etching time was 80 s. The pore etching current density was 250 mA / cm 2 , the pore charge density is 20C / cm 2 The surface of the aluminum foil treated above was subjected to scanning electron microscope morphology and pore size distribution statistics, see Figure 2 .

[0029] Example 1

[0030] Prepare a nitric acid solution with a concentration of 1 mol / L and heat it to 60°C. Then, soak an electrolytic capacitor high-voltage anode aluminum foil with a thickness of 120 μm, a purity of 99.99 wt.%, a {100} texture occupancy of more than 97%, and containing trace Cu, Si, and Fe elements in the nitric acid solution for 4 minutes and then take it out. Wash the surface of the aluminum foil with deionized water and dry it at room temperature.

[0031] Prepare 1 liter of 3 wt.% silane solution, add 0.5 mmol of Ce(NO3)3 corrosion inhibitor, and heat the solution to 60°C. Then soak the aluminum foil polished with the acid solution for 5 minutes, then take it out and dry it directly at room temperature.

[0032] Prepare a pore-forming solution with a concentration of 3.5 mol / L H2SO4+0.7 mol / L HCl and heat it to 70°C. Place the pretreated aluminum foil in it and pass direct current to etch and pore. The pore-forming time is 80 s and the pore-forming current density is 250 mA / cm 2 , the pore charge density is 20C / cm 2 .

[0033] Example 2

[0034] Prepare a nitric acid solution with a concentration of 1.0 mol / L and heat it to 70°C. Then, immerse an electrolytic capacitor high-voltage anode aluminum foil with a thickness of 120 μm, a purity of 99.99 wt.%, a {100} texture occupancy of more than 97%, and containing trace Cu, Si, and Fe elements in the nitric acid solution for 6 minutes and then take it out. Wash the surface of the aluminum foil with deionized water and dry it at room temperature.

[0035] Prepare 1 liter of 3 wt.% silane solution, add 1.0 mmol of Ce(NO3)3 corrosion inhibitor, and heat the solution to 60°C. Then soak the aluminum foil polished with the acid solution for 10 minutes, then take it out and dry it directly at room temperature.

[0036] Prepare a pore-forming solution with a concentration of 3.5 mol / L H2SO4+0.7 mol / L HCl and heat it to 70°C. Place the pretreated aluminum foil in it and pass direct current to etch and pore. The pore-forming time is 80 s and the pore-forming current density is 250 mA / cm 2 , the pore charge density is 20C / cm 2 .

[0037] Example 3

[0038] A nitric acid solution with a concentration of 1.5 mol / L was prepared and heated to 60°C. Then, an electrolytic capacitor high-voltage anode aluminum foil with a thickness of 120 μm, a purity of 99.99 wt.%, a {100} texture occupancy of more than 97%, and containing trace Cu, Si, and Fe elements was soaked in the nitric acid solution for 4 minutes and then taken out. The surface of the aluminum foil was cleaned with deionized water and dried at room temperature.

[0039] Prepare 1 liter of 5 wt.% silane solution, add 0.5 mmol of Na2MoO4 corrosion inhibitor, and heat the solution to 60° C. Then soak the aluminum foil polished with the acid solution for 15 minutes, and then take it out and dry it directly at room temperature.

[0040] Prepare a pore-forming solution with a concentration of 3.5 mol / L H2SO4+0.7 mol / L HCl and heat it to 70°C. Place the pretreated aluminum foil in it and pass direct current to etch and pore. The pore-forming time is 80 s and the pore-forming current density is 250 mA / cm 2 , the pore charge density is 20C / cm 2 .

[0041] Example 4

[0042] Prepare a nitric acid solution with a concentration of 0.5 mol / L and heat it to 50°C. Then, soak an electrolytic capacitor high-voltage anode aluminum foil with a thickness of 120 μm, a purity of 99.99 wt.%, a {100} texture occupancy of more than 97%, and containing trace Cu, Si, and Fe elements in the nitric acid solution for 10 minutes and then take it out. Wash the surface of the aluminum foil with deionized water and dry it at room temperature.

[0043] Prepare 1 liter of 5 wt.% polyethylene glycol solution, add 0.5 mmol of Na2MoO4 corrosion inhibitor, and heat the solution to 60° C. Then soak the aluminum foil polished with the acid solution for 10 minutes, and then take it out and dry it directly at room temperature.

[0044] Prepare a pore-forming solution with a concentration of 3.5 mol / L H2SO4+0.7 mol / L HCl and heat it to 70°C. Place the pretreated aluminum foil in it and pass direct current to etch and pore. The pore-forming time is 80 s and the pore-forming current density is 250 mA / cm 2 , the pore charge density is 20C / cm 2 .

[0045] Example 5

[0046] Prepare a nitric acid solution with a concentration of 1 mol / L and heat it to 70°C. Then, soak an electrolytic capacitor high-voltage anode aluminum foil with a thickness of 120 μm, a purity of 99.99 wt.%, a {100} texture occupancy of more than 97%, and containing trace Cu, Si, and Fe elements in the nitric acid solution for 6 minutes and then take it out. Wash the surface of the aluminum foil with deionized water and dry it at room temperature.

[0047] Prepare 1 liter of 3 wt.% silane solution, add 1 mmol of Na2MoO4 corrosion inhibitor and 1 mmol of Ce(NO3)3 corrosion inhibitor respectively, and heat the solution to 60°C. Then soak the aluminum foil polished with the acid solution in it for 10 minutes, and then take it out and dry it directly at room temperature.

[0048] Prepare a pore-forming solution with a concentration of 3.5 mol / L H2SO4+0.7 mol / L HCl and heat it to 70°C. Place the pretreated aluminum foil in it and pass direct current to etch and pore. The pore-forming time is 80 s and the pore-forming current density is 250 mA / cm 2 , the pore charge density is 20C / cm 2 . In addition, the present invention makes a scanning electron microscope morphology image after corroding and pore-forming the aluminum foil assembled with an organic polymer film doped with a corrosion inhibitor after polishing, and makes statistics on the pore size distribution of the surface tunnel holes, as shown in Figure 3 for details. The scanning electron microscope photo can directly show the state of the pore distribution on the aluminum foil surface, and the pore size distribution statistics can illustrate the concentration degree of the corrosion pores, and also reflect the uniformity of the corrosion holes. In comparative example 1, the surface pores of the aluminum foil without surface pretreatment are extremely uneven, a large number of blank areas appear on the surface of the aluminum foil, and there is a serious aggregation of tunnel holes in the pore area. In comparative example 2, the uniformity of the distribution of tunnel holes on the surface of the aluminum foil after surface chemical deposition of tin crystal nuclei has been improved to a certain extent, but there are still blank areas and obvious parallel holes. In Example 5, the distribution of tunnel holes on the surface of the aluminum foil after the two-step combined surface pretreatment is uniform, there is no obvious blank area, and the distance between the tunnel holes is very suitable and almost consistent. The tunnel holes formed by the corrosion pores on the surface of the aluminum foil need to have a moderate pore size, a concentrated pore size distribution, and a surface density as high as possible. Compared with the statistical results of the pore size distribution of the surface tunnel holes without pretreatment and after chemical deposition of tin crystal nuclei on the surface, the tunnel pore size after the two-step combined surface pretreatment of the present invention is concentrated in 0.8-1.6μm, which is moderate in size. The tunnel holes will not be blocked during the chemical formation process due to too small pore size, nor will they cause pore merging and collapse due to too large pore size, thereby improving the uniformity of pore formation. On the surface of aluminum foil without surface pretreatment, the pore size distribution is very wide and very dispersed, and the number of tunnel holes with pore size less than 0.8μm still accounts for a large proportion. These tunnel holes are easily blocked during the chemical formation process. On the other hand, the tunnel hole aggregation phenomenon is serious, which is easy to cause pore merging during the hole expansion process, thereby causing the aluminum foil specific volume to decrease and the performance to decrease.

[0049] Table 1 is a table of the average diameter, average area, tunnel hole density and specific surface area of ​​the tunnel holes on the surface of the aluminum foil after the high-voltage anode aluminum foil in the comparative example and the embodiment is corroded and pore-forming. It can be seen that the density and specific surface area of ​​the tunnel holes on the surface of the aluminum foil after the two-step combined pretreatment of the present invention are greatly improved compared with the comparative example, and the pore size distribution is also more concentrated.

[0050] Table 1 Parameters of tunnel holes on the surface of perforated aluminum foil in comparative examples and embodiments

[0051]

Claims

1. A method for pretreating the surface of high-voltage anode aluminum foil corrosion holes, characterized in that: The surface treatment of high voltage anode aluminum foil is carried out by a two-step combined pretreatment method. The specific steps are as follows: Step 1: polishing the surface of the high voltage anode aluminum foil in an acid solution; Step 2: Assemble an organic polymer film doped with a corrosion inhibitor on the polished aluminum foil surface.

2. The method for pretreating the surface of high-voltage anode aluminum foil corrosion holes according to claim 1, characterized in that: The surface polishing described in step 1 is to immerse the aluminum foil in an acidic solution for chemical polishing, wherein the acidic solution is a 0.1-1.5 mol / L HNO3 solution, the polishing solution temperature is 25-80°C, and the processing time is 0.5-10 min.

3. The method for pretreating the surface of high-voltage anode aluminum foil corrosion holes according to claim 1, characterized in that: The implementation method of the surface assembly of the organic polymer film doped with the corrosion inhibitor in step 2 is to mix the corrosion inhibitor and the organic polymer to prepare an aqueous solution, and then immerse the aluminum foil in the aqueous solution to perform surface self-assembly to form the film.

4. The method for pretreating the surface of high-voltage anode aluminum foil corrosion holes according to claim 1, characterized in that: The corrosion inhibitor described in step 2 is a salt selected from the group consisting of cerium salt, molybdate, tungstate, vanadate, borate, phosphate, and silicate, or a mixture of any two or more salts.

5. The method for pretreating the surface of high-voltage anode aluminum foil corrosion holes according to claim 1, characterized in that: The organic polymer described in step 2 is one or a combination of silane, polyethylene glycol, polyaniline, imidazoline acrylate, imidazoline oleate, 8-hydroxyquinoline, benzotriazole, and oleic acid.

6. The method for pretreating the surface of high-voltage anode aluminum foil corrosion holes according to claim 3, characterized in that: The concentration of the corrosion inhibitor in the aqueous solution is 0.1-2.0 mmol / L, and the concentration of the organic polymer in the aqueous solution is 0.1-5 wt.%.

7. A method for pretreating the surface of high-voltage anode aluminum foil corrosion holes according to claim 3, characterized in that: The temperature of the surface self-assembly solution is 25-80 °C, and the immersion time is 0.5-15 min.

Citation Information

Cited By

  • Method for pretreating aluminum foil before electrochemical corrosion hole forming so as to improve distribution uniformity of corrosion holes

    CN121514130A