Environmentally friendly impermeable concrete and preparation method thereof
By increasing the amount of fly ash in environmentally friendly anti-seepage concrete and using calcium hydroxide and specific admixtures to stimulate fly ash activity, the problem of poor fly ash consumption effect is solved, and high strength and good anti-seepage performance is achieved. Concrete reduces environmental pollution.
Patent Information
- Application Number
- CN202310336943.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-03-31
AI Technical Summary
The amount of fly ash in existing environmentally friendly concrete is low, resulting in poor fly ash consumption effect and affecting the environment and concrete performance.
The environmental protection is formed by using up to 50% fly ash dosage and the addition of calcium hydroxide to stimulate the activity of fly ash, combined with admixtures made of sodium gluheptanoate, tartaric acid, sodium citrate and sodium lignin sulfonate. Anti-seepage concrete mixing materials to improve fly ash consumption, compactness and anti-seepage properties of concrete.
It significantly increases the consumption of fly ash, improves the early and late strength of concrete, improves the permeability resistance, reduces environmental pollution, and ensures the quality of concrete.
Abstract
Description
Technical Field
[0001] The invention relates to the field of concrete, and in particular to an environmentally friendly anti-seepage concrete and a preparation method thereof. Background Art
[0002] Environmentally friendly concrete refers to concrete materials with fly ash added. Fly ash is mainly tiny ash particles discharged during the combustion of coal. Every ton of coal burned will produce about 250-300kg of fly ash. If a large amount of fly ash is not treated, it will cause serious air pollution. Therefore, applying fly ash to concrete is a major method of treating fly ash.
[0003] However, existing research shows that the fly ash content is generally around 20-30%. If the fly ash content is too high, it will affect the performance of concrete. Therefore, the fly ash content is relatively low. Although the current amount of concrete used is large, the output of fly ash is also very large. The effect of consuming fly ash through the preparation of concrete is relatively general, so there is still room for improvement. Summary of the invention
[0004] In order to improve the effect of consuming fly ash, the present application provides an environmentally friendly anti-seepage concrete and a preparation method thereof.
[0005] In the first aspect, the present application provides an environmentally friendly impermeable concrete, which adopts the following technical solution:
[0006] An environmentally friendly impermeable concrete is made of a concrete mixture, wherein the concrete mixture includes the following components in parts by mass: 100 parts of water;
[0007] 180-190 parts of cement;
[0008] 180-190 parts of fly ash;
[0009] 450-470 parts of fine aggregate;
[0010] 650-670 parts of coarse aggregate;
[0011] Calcium hydroxide 5.4-5.7 parts;
[0012] Admixture 2.1-2.4 parts;
[0013] The additive is a compound of sodium glucoheptonate, tartaric acid, sodium citrate and sodium lignin sulfonate.
[0014] By adopting the above technical solution, the fly ash content is as high as 50%, which is a great improvement over the 20%-30% content in the existing environmentally friendly concrete, so that the fly ash consumption is greatly increased, so that the fly ash can be better consumed, and the effect of consuming fly ash is improved, thereby better reducing the environmental pollution caused by fly ash accumulation, which is more environmentally friendly.
[0015] Adding a large amount of fly ash can better fill the pores of concrete, improve the density of concrete, and make the concrete have better anti-permeability properties.
[0016] By adding calcium hydroxide as a fly ash activation activator, the fly ash can fully generate hydraulic substances such as hydrated calcium silicate, hydrated calcium aluminate and hydrated calcium sulfoaluminate, thereby increasing the early and late strengths of the concrete, making the physical properties of the produced concrete better and not easily affecting the quality of the concrete.
[0017] Since calcium hydroxide is added to the formula, hydration will be accelerated, thereby generating more hydration heat, making the concrete more prone to the appearance of a large number of capillaries, thereby reducing the concrete's impermeability. The admixture formed by adding sodium glucoheptonic acid, tartaric acid, sodium citrate, and sodium lignin sulfonate has a better retarding effect, making the generation of hydration heat more stable, reducing the generation of capillaries, and increasing the density of concrete, thereby better improving the concrete's impermeability.
[0018] Preferably, the concrete mixture comprises the following components in parts by weight:
[0019] 100 parts water;
[0020] Cement 184-186 parts;
[0021] Fly ash 184-186 parts;
[0022] 455-465 parts of fine aggregate;
[0023] 655-665 parts of coarse aggregate;
[0024] Calcium hydroxide 5.52-5.58 parts;
[0025] 2.22-2.28 parts of admixture.
[0026] By adopting the above technical solution and specifically selecting the proportion range of each component, the obtained concrete has higher strength, better impermeability and better quality, and a high-quality concrete material can be produced while consuming a large amount of fly ash.
[0027] Preferably, the mass ratio of the cement, fly ash and calcium hydroxide is 1:1:0.03.
[0028] By adopting the above technical solution and specifically selecting the ratio of cement, fly ash and calcium hydroxide, the effect of stimulating the activity of fly ash is better and the quality of the prepared concrete is better.
[0029] Preferably, the mass ratio of the sodium glucoheptonate, tartaric acid, sodium citrate and sodium lignin sulfonate is 0.1:0.05:0.2:0.25.
[0030] By adopting the above technical scheme and specifically selecting the mass ratio of sodium glucoheptonate, tartaric acid, sodium citrate and sodium lignin sulfonate, the retarding effect is more appropriate and will not affect the performance of the concrete. At the same time, the hydration heat can be controlled to be generated more smoothly, and it is not easy to cause severe thermal expansion and contraction due to local heating and the appearance of a large number of capillaries, thereby better improving the density of the concrete and the anti-permeability performance.
[0031] In a second aspect, the present application provides a method for preparing environmentally friendly impermeable concrete, which adopts the following technical solution:
[0032] A method for preparing the above-mentioned environmentally friendly impermeable concrete comprises the following steps:
[0033] Step 1) taking part of the water and mixing with the admixture, reducing the pressure to 0.01-0.02 MPa, raising the temperature to 150-160° C., rotating at 120-160 r / min, stirring for 30-45 min, and cooling to room temperature to obtain an admixture solution;
[0034] Step 2), taking part of the water and mixing with calcium hydroxide, adding fly ash, stirring for 30-45 minutes, and obtaining fly ash mixture;
[0035] Step 3), taking the remaining water and mixing it with cement to obtain a cement mixture;
[0036] Step 4), mixing the admixture solution, the fly ash solution and the cement solution to form a premix;
[0037] Step 5), adding fine aggregate and coarse aggregate to the premix and mixing to obtain a concrete mixture;
[0038] Step 6), pouring the concrete mixture into a mold, curing, and demoulding to obtain environmentally friendly and impermeable concrete.
[0039] By adopting the above technical scheme and through special treatment of the admixture, the admixture not only has a good retarding effect, but also can improve the heat dissipation effect of concrete, so that the hydration heat energy can be discharged more timely, thereby better reducing the phenomenon of capillaries caused by expansion of concrete, thereby making the concrete denser and more impermeable.
[0040] By mixing calcium hydroxide with fly ash, the activity of fly ash can be better and targetedly stimulated. By adding fly ash that has been activated, the early strength of concrete can be improved, thereby improving the early strength of concrete to better adapt to engineering applications with high requirements for early strength.
[0041] Preferably, in step 1), the mass ratio of water mixed with the admixture to the mass ratio of the admixture is 1:1-1.2.
[0042] By adopting the above technical solution, by specifically selecting the mass ratio of water and admixture, controlling the concentration of the admixture solution, and under special conditions, the various raw materials can better cooperate with each other, thereby achieving a better effect of improving the heat dissipation performance of the concrete hydration process.
[0043] Preferably, in step 2), the ratio of the mass of water mixed with fly ash to the mass of fly ash is 1:5-5.2.
[0044] By adopting the above technical scheme and specifically selecting the mass ratio of fly ash to water, the concentration of the alkaline solution is made higher, thereby better stimulating the activity of the fly ash. After the fly ash is activated, it is mixed with other raw materials to better improve the early strength of the concrete and has a wider applicability.
[0045] Preferably, in step 2), the temperature is kept at 60-65° C. during stirring.
[0046] By adopting the above technical solution, by stirring at 60-65°C and increasing the temperature, a better activation effect of fly ash is achieved. The activated fly ash has higher activity and is more conducive to improving the early strength of concrete.
[0047] In summary, this application has the following beneficial effects:
[0048] 1. Since the present application adds calcium hydroxide as a fly ash activation activator, the fly ash is fully converted into hydraulic substances such as hydrated calcium silicate, hydrated calcium aluminate and hydrated calcium sulfoaluminate, thereby increasing the early strength and late strength of the concrete, making the physical properties of the prepared concrete better and not easily affecting the quality of the concrete.
[0049] 2. In the present application, it is preferred to add an admixture formed by compounding sodium glucoheptonic acid, tartaric acid, sodium citrate and sodium lignin sulfonate, which has a good retarding effect, makes the generation of hydration heat more stable, reduces the generation of capillaries, and improves the density of concrete, thereby better improving the anti-permeability performance of concrete.
[0050] 3. The method of the present application reduces the pressure and increases the temperature of the admixture, so that the admixture not only has a good retarding effect, but also can improve the heat dissipation effect of the concrete, so that the hydration heat energy can be discharged more promptly, thereby better reducing the phenomenon of capillaries caused by expansion of the concrete, thereby making the concrete denser and more impermeable. DETAILED DESCRIPTION
[0051] The present application is further described in detail below with reference to the embodiments.
[0052] Example 1
[0053] The invention discloses an environmentally friendly anti-seepage concrete, which is made from concrete mixture.
[0054] Concrete mix consists of the following components:
[0055] Water, cement, fly ash, fine aggregate, coarse aggregate, calcium hydroxide, admixtures.
[0056] Among them, cement is silicate cement with the standard of P.O45.5.
[0057] Among them, the fly ash is first-grade fly ash.
[0058] Among them, the fine aggregate is 20 mesh river sand.
[0059] Among them, the coarse aggregate is basalt crushed stone with an average particle size of 10mm.
[0060] The additive is a compound of sodium glucoheptonate, tartaric acid, sodium citrate and sodium lignin sulfonate.
[0061] Among them, sodium glucoheptonate is commercially available, CAS: 10094-62-9.
[0062] The tartaric acid is commercially available, CAS: 526-83-0.
[0063] Among them, sodium citrate is commercially available, CAS: 68-04-2.
[0064] Among them, sodium lignin sulfonate is commercially available, CAS: 8061-51-6.
[0065] In Examples 1-5, the specific input amounts of the components of the concrete mixture are shown in Table 1.
[0066] Table 1
[0067] Example 1 Example 2 Example 3 Example 4 Example 5 water 100 100 100 100 100 cement 180 184 185 186 190 Fly ash 180 184 185 186 190 river sand 450 455 460 465 470 gravel 650 655 660 665 670 Calcium hydroxide 5.4 5.52 5.55 5.58 5.7 Sodium Gluceptate 0.35 0.37 0.375 0.38 0.4 tartaric acid 0.175 0.185 0.1875 0.19 0.2 Sodium Citrate 0.7 0.74 0.75 0.76 0.8 Sodium lignin sulfonate 0.875 0.925 0.9375 0.95 1
[0068] In Examples 1-5, the method for preparing the environmentally friendly impermeable concrete comprises the following steps:
[0069] Step 1) taking part of the water and mixing with the admixture, the mass ratio of water to the admixture is 1:1, reducing the pressure to 0.01 MPa, raising the temperature to 150° C., condensing and refluxing, rotating speed 120 r / min, stirring for 45 min, cooling to room temperature, and obtaining an admixture solution;
[0070] Step 2), taking part of the water and mixing with calcium hydroxide, and then adding fly ash, the mass ratio of water to fly ash is 1:5, the rotation speed is 60r / min, and stirring at room temperature for 30min to obtain fly ash mixture;
[0071] Step 3), taking the remaining water and mixing it with cement, rotating speed 90r / min, stirring for 3min to obtain cement mixture;
[0072] Step 4), mixing the admixture solution, fly ash solution and cement solution at a speed of 60 r / min and stirring for 1 min to form a premix;
[0073] Step 5), add fine aggregate and coarse aggregate to the premix, rotate at 60r / min, stir for 8min, and mix to obtain a concrete mixture; Step 6), pour the concrete mixture into a mold, sprinkle water for curing for 3d, demould, and stand for curing for 28d to obtain environmentally friendly anti-seepage concrete.
[0074] Example 6
[0075] An environmentally friendly impermeable concrete, compared with Example 3, the only difference is:
[0076] In the preparation method of environmentally friendly impermeable concrete:
[0077] Step 1), taking part of the water and mixing with the admixture, the mass ratio of water to the admixture is 1:1.2, reducing the pressure to 0.02MPa, raising the temperature to 160°C, condensing and refluxing, rotating speed 160r / min, stirring for 30min, cooling to room temperature, and obtaining an admixture solution;
[0078] Step 2), taking part of the water and mixing with calcium hydroxide, and then adding fly ash, the mass ratio of water to fly ash is 1:5.2, the rotation speed is 60r / min, and stirring at room temperature for 45min to obtain fly ash mixture;
[0079] The remaining steps are consistent with Example 3.
[0080] Example 7
[0081] An environmentally friendly impermeable concrete, compared with Example 3, the only difference is:
[0082] In the preparation method of environmentally friendly impermeable concrete:
[0083] Step 2), taking part of the water and mixing with calcium hydroxide, and then adding fly ash, the mass ratio of water to fly ash is 1:5, the speed is 60r / min, and the temperature is kept at 60°C and stirred for 30min to obtain fly ash mixture;
[0084] Example 8
[0085] An environmentally friendly impermeable concrete, compared with Example 3, the only difference is:
[0086] In the preparation method of environmentally friendly impermeable concrete:
[0087] Step 2), taking part of the water and mixing with calcium hydroxide, and then adding fly ash, the mass ratio of water to fly ash is 1:5, the speed is 60r / min, and the temperature is kept at 65°C and stirred for 30min to obtain fly ash mixture;
[0088] Comparative Example 1
[0089] An environmentally friendly impermeable concrete, compared with Example 3, the only difference is:
[0090] In concrete mixture, sodium gluconate is used in equal amounts to replace sodium glucoheptonate.
[0091] Among them, sodium gluconate is commercially available, CAS: 527-07-1.
[0092] Comparative Example 2
[0093] An environmentally friendly impermeable concrete, compared with Example 3, the only difference is:
[0094] In concrete mix, an equal amount of glucose is used instead of tartaric acid.
[0095] Glucose was commercially available.
[0096] Comparative Example 3
[0097] An environmentally friendly impermeable concrete, compared with Example 3, the only difference is:
[0098] In concrete mixture, an equal amount of white sugar is used to replace sodium citrate.
[0099] Among them, white sugar is commercially available.
[0100] Comparative Example 4
[0101] An environmentally friendly impermeable concrete, compared with Example 3, the only difference is:
[0102] In concrete mixture, calcium lignin sulfonate is used in equal amounts to replace sodium lignin sulfonate.
[0103] Calcium lignin sulfonate is commercially available, CAS: 8061-52-7.
[0104] Comparative Example 5
[0105] An environmentally friendly impermeable concrete, compared with Example 3, the only difference is:
[0106] In concrete mix, calcium hydroxide is replaced by an equal amount of fine aggregate.
[0107] In the preparation method of environmentally friendly impermeable concrete:
[0108] Step 2), taking part of the water and mixing with the fly ash, the mass ratio of water to fly ash is 1:5, the rotation speed is 60r / min, and stirring at room temperature for 30min to obtain the fly ash mixture;
[0109] Comparative Example 6
[0110] An environmentally friendly impermeable concrete, compared with Example 3, the only difference is:
[0111] In the preparation method of environmentally friendly impermeable concrete:
[0112] Step 1) taking part of the water and mixing with the admixture, the mass ratio of water to the admixture is 1:1, the speed is 120r / min, stirring for 45min, and cooling to room temperature to obtain an admixture solution;
[0113] Comparative Example 7
[0114] An environmentally friendly impermeable concrete, compared with Example 3, the only difference is:
[0115] In concrete mix:
[0116] The amount of cement input is adjusted to 259 kg.
[0117] The amount of fly ash input is adjusted to 111 kg.
[0118] Experiment 1
[0119] According to the "Standard for Test Methods of Mechanical Properties of Ordinary Concrete GB / T50081-2016", the 7d compressive strength, 28d compressive strength and 60d compressive strength of the environmentally friendly impermeable concrete of each embodiment and comparative example were tested. 67.6MPa
[0120] Experiment 2
[0121] The impermeability grade of the environmentally friendly impermeable concrete of each embodiment and comparative example was tested according to the "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete GB / T50082-2009".
[0122] The specific test data of Experiments 1 and 2 are shown in Table 2.
[0123] Table 2
[0124] 7d compressive strength 28d compressive strength 60d compressive strength Impermeability grade Example 1 53.4 70.1 95.9 >P12 Example 2 53.5 70.3 95.4 >P12 Example 3 53.8 70.4 97.6 >P12 Example 4 53.7 70.2 96.8 >P12 Example 5 53.6 70.1 95.9 >P12 Example 6 53.9 70.2 97.9 >P12 Example 7 56.2 71.6 96.3 >P12 Example 8 56.4 71.8 95.9 >P12 Comparative Example 1 53.9 69.6 97.0 P10 Comparative Example 2 53.8 69.7 97.3 P10 Comparative Example 3 53.7 69.5 96.7 P10 Comparative Example 4 54.4 69.8 97.6 P10 Comparative Example 5 39.9 63.8 73.1 >P12 Comparative Example 6 53.0 69.9 95.9 P12 Comparative Example 7 53.3 67.6 88.2 P12
[0125] According to the data comparison in Table 2, by adding calcium hydroxide and an admixture formed by mixing sodium glucoheptonate, tartaric acid, sodium citrate and sodium lignin sulfonate, the fly ash content in the concrete reaches 50%, and the obtained concrete has excellent performance, and is even stronger than the concrete with 30% content, and has better impermeability and comprehensive performance. It can also better consume fly ash, reduce environmental pollution, and is more environmentally friendly and green.
[0126] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. An environmentally friendly impermeable concrete, Features: Made of concrete mixture, the concrete mixture includes the following components in parts by weight: 100 parts water; 180-190 parts of cement; 180-190 parts of fly ash; 450-470 parts of fine aggregate; 650-670 parts of coarse aggregate; Calcium hydroxide 5.4-5.7 parts; Admixture 2.1-2.4 parts; The additive is a compound of sodium glucoheptonate, tartaric acid, sodium citrate and sodium lignin sulfonate; The mass ratio of cement, fly ash and calcium hydroxide is 1:1:0.03; The mass ratio of the sodium glucoheptonate, tartaric acid, sodium citrate and sodium lignin sulfonate is 0.1:0.05:0.2:0.
25.
2. The environmentally friendly impermeable concrete according to claim 1, Features: The concrete mixture comprises the following components in parts by weight: 100 parts water; Cement 184-186 parts; Fly ash 184-186 parts; 455-465 parts of fine aggregate; 655-665 parts of coarse aggregate; Calcium hydroxide 5.52-5.58 parts; 2.22-2.28 parts of admixture.
3. A method for preparing the environmentally friendly impermeable concrete according to claim 1 or 2, Features: The following steps are involved: Step 1) Take part of the water and mix with the admixture, reduce the pressure to 0.01-0.02MPa, raise the temperature to 150-160°C, rotate at 120-160r / min, stir for 30-45min, and cool to room temperature to obtain the admixture solution; Step 2), taking part of the water and mixing with calcium hydroxide, adding fly ash, stirring for 30-45 minutes, and obtaining fly ash mixture; Step 3), taking the remaining water and mixing it with cement to obtain a cement mixture; Step 4), mixing the admixture solution, the fly ash mixture and the cement mixture to form a premix; Step 5), adding fine aggregate and coarse aggregate to the premix and mixing to obtain a concrete mixture; Step 6), pouring the concrete mixture into the mold, curing and demoulding to obtain environmentally friendly and impermeable concrete.
4. A method for preparing environmentally friendly impermeable concrete according to claim 3, Features: In the step 1), the mass ratio of the water mixed with the admixture to the mass ratio of the admixture is 1:1-1.
2.
5. A method for preparing environmentally friendly impermeable concrete according to claim 4, Features: In the step 2), the ratio of the mass of water mixed with the fly ash to the mass of the fly ash is 1:5-5.
2.
6. A method for preparing environmentally friendly impermeable concrete according to claim 5, Features: In the step 2), the temperature is kept at 60-65° C. during stirring.