A method for preparing aging-resistant and wear-resistant water-based suede microfiber leather

By using composite modified nanopowder and specific cross-linking agent in water-based suede microfiber leather, the problem of difficulty in achieving both aging resistance and wear resistance in the existing technology is solved, and the wear resistance and wear resistance of microfiber leather are significantly improved. Aging resistance.

CN116815517BActive Publication Date: 2024-10-22FUJIAN ZHONGYU WATERBORNE MICROFIBER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310823928.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-06
Publication Date
2024-10-22
Estimated Expiration
2043-07-06

AI Technical Summary

Technical Problem

It is difficult to achieve both aging resistance and wear resistance in water-based suede microfiber leather with the existing technology, and usually only one of the excellent properties can be achieved.

Method used

Using composite modified nanopowders, including modified nanocalcium carbonate and nanotitanium dioxide, the mechanical properties and wear properties of microfiber leather are improved through the doping of modified materials, and combined with specific cross-linking agents and catalysts, a resistant material is prepared. Aging and wear-resistant water-based suede microfiber leather.

Benefits of technology

It significantly improves the aging and wear resistance of water-based suede microfiber leather, improves the micromorphology and overall uniformity of the composite material, slows down the plastic deformation and wear of the material, and enhances the bonding strength and surface stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004324387690000121
    Figure BDA0004324387690000121
Patent Text Reader

Abstract

The present invention discloses a method for preparing an aging-resistant and wear-resistant water-based suede microfiber leather, the steps of which include: (1) preparation of a padding solution: adding water and a penetrant to an aqueous polyurethane solution and stirring evenly; wherein the raw materials of the aqueous polyurethane include: polyoxypropylene glycol, polyoxypropylene glycol, polyethylene adipate polyol, isophorone diisocyanate, a hydrophilic chain extender, a crosslinking agent, and a composite modified nanopowder. (2) Padding: immersing the cut microfiber into a pre-prepared aqueous polyurethane padding solution, passing the fabric through a padder after sufficient dipping, and drying it at 160-180°C and keeping it for 6-10 minutes. The present invention uses the aforementioned method for preparing a water-based suede microfiber leather, adds a composite modified nanopowder, and takes the nano-modified material as the core to prepare a microfiber leather, which can effectively improve the aging resistance and wear resistance of the water-based suede microfiber leather.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water-based suede microfiber leather, and in particular to a method for preparing aging-resistant and wear-resistant water-based suede microfiber leather. Background Art

[0002] Superfine fiber synthetic leather is very close to natural leather in appearance, feel and internal structure. It is the most ideal substitute for natural leather. Its market share increases by 20% every year. With the continuous improvement of technology, medium and high-end superfine fiber synthetic leather series products emerge in an endless stream, and the application field continues to expand. Water-based polyurethane padding liquid has little impact on the environment and human health, which is conducive to improving the competitiveness of products in domestic and foreign markets, plays a positive role in reducing pollution and ecological protection, and can also avoid the harm of organic solvent residues to the human body. Based on the different market demands for this kind of superfine fiber synthetic leather, the research directions are also different.

[0003] Patent CN106223058A discloses a method for making a water-based suede microfiber leather that is resistant to light aging and wear, characterized in that the steps mainly include (1) preparing slurry-(2) impregnation and extrusion-(3) pre-solidification and drying-(4) main solidification and drying-(5) alkali reduction-(6) dyeing and raising; Step (1) preparing slurry: using water-based polycarbonate polyurethane resin as the main body to prepare a compounding liquid with a viscosity of 450±100cps, the composition of each component of the compounding liquid is as follows in weight percentage: 100 parts of water-based polycarbonate polyurethane resin, 60-80 parts of water, 2.4-3.5 parts of thickener, 1.6-2.4 parts of bridging agent, 0.8-1.4 parts of electrolyte, and 2.0-3.0 parts of penetrant. The water-based suede microfiber leather prepared by the present invention meets the requirements of light aging and wear resistance, and overcomes the shortcomings of suede products that are easy to fade and wear. At the same time, compared with traditional suede microfiber leather, it retains the breathability characteristics while meeting the physical properties of low odor and low VOC, achieving truly clean and environmentally friendly production, and increasingly meeting environmental protection requirements.

[0004] Patent CN115613371A relates to a method for preparing a highly wear-resistant waterborne polyurethane microfiber base fabric, comprising the following steps: (1) the sea-island fibers are combed, laid and needled to form a non-woven fabric; (2) the non-woven fabric is impregnated with a waterborne polyurethane emulsion, and a waterborne polyurethane sea-island fiber base fabric is obtained by a two-impregnation curing process; (3) the waterborne polyurethane sea-island fiber base fabric is subjected to fiber opening and napping to obtain a highly wear-resistant waterborne polyurethane microfiber base fabric; the sea phase of the sea-island fiber is a water-soluble polyester WSPET, and the sea phase residual rate is controlled to be 0.4-1% during the fiber opening process. The highly wear-resistant waterborne polyurethane microfiber base fabric prepared by the present invention has a wear amount of 5-12 mg after 35,000 tests according to GB / T 21196.2-2007 standard. The present invention uses water-soluble polyester as the sea phase, and by controlling the sea phase residual rate to be 0.4-1% after fiber opening, the Martin wear resistance of the base fabric is significantly improved without affecting the surface napping effect.

[0005] However, the prior art only achieves one of the wear resistance or aging resistance, or cannot achieve excellent performance of both of the above properties. Based on this, the present application provides a method for preparing aging-resistant and wear-resistant water-based suede microfiber leather. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing an aging-resistant and wear-resistant water-based suede microfiber leather. By innovating the raw materials and methods, adding composite modified nanopowders, and taking nano-modified materials as the core, microfiber leather is prepared to effectively improve the aging resistance and wear resistance of the water-based suede microfiber leather.

[0007] A method for preparing aging-resistant and wear-resistant water-based suede microfiber leather, comprising the following steps:

[0008] (1) Preparation of padding solution: Add water and penetrant to aqueous polyurethane solution and stir evenly;

[0009] Wherein, the raw materials of the waterborne polyurethane include:

[0010] Polyoxypropylene glycol, polyoxypropylene glycol, polyethylene adipate polyol, isophorone diisocyanate, chain extender, crosslinking agent, catalyst and composite modified nano powder.

[0011] (2) Padding: The cut microfibers are immersed in the prepared aqueous polyurethane padding solution. After being fully impregnated, the fabrics are passed through a padding machine and dried at 160-180°C for 6-10 minutes.

[0012] Furthermore, the cross-linking agent comprises castor oil and polyoxypropylene glycol in a mass ratio of 1:1-2.

[0013] Furthermore, the chain extender includes 1,4-butanediol and / or 1,3-propylene glycol.

[0014] Furthermore, the catalyst includes dibutyltin dilaurate.

[0015] Furthermore, the rolling rate during the rolling process is 120-150%.

[0016] Furthermore, the raw materials of the waterborne polyurethane include:

[0017] 70-90 parts of polyoxypropylene glycol,

[0018] 80-100 parts of polyoxypropylene glycol,

[0019] 120-200 parts of polyethylene adipate polyol,

[0020] 80-110 parts of isophorone diisocyanate,

[0021] Chain extender 15-20 parts,

[0022] 6-8 parts of cross-linking agent,

[0023] 1-3 parts of catalyst,

[0024] 15-30 parts of composite modified nano powder.

[0025] Furthermore, the composite nano-modified powder includes modified nano-calcium carbonate and / or nano-titanium dioxide.

[0026] Furthermore, the preparation method of the modified nano-calcium carbonate comprises: adding anhydrous ethanol and a silane coupling agent to the nano-calcium carbonate, stirring, and ultrasonicating for 30-60 minutes to obtain the modified nano-calcium carbonate.

[0027] Furthermore, the silane coupling agent comprises γ-aminopropyltriethoxysilane and γ-glycidyloxypropyltrimethoxysilane in a mass ratio of 1:1.

[0028] Furthermore, the preparation method of the silane coupling agent modified nano titanium dioxide comprises: mixing anhydrous ethanol, deionized water and a silane coupling agent, hydrolyzing for 30-45 minutes to obtain a mixed solution, mixing the nano titanium dioxide and the anhydrous ethanol for ultrasonic dispersion, then adding the mixed solution, maintaining at 85-90° C. for 2-3 hours, filtering, washing and drying to obtain the silane coupling agent modified nano titanium dioxide.

[0029] Furthermore, the weight ratio of the anhydrous ethanol, deionized water and silane coupling agent is (60-70): (5-6): (12-18).

[0030] Furthermore, the weight ratio of the nano titanium dioxide to anhydrous ethanol is 1:(12-15).

[0031] Furthermore, the mass of the silane coupling agent is 10-20% of the nano titanium dioxide.

[0032] Furthermore, the silane coupling agent comprises methyltriethoxysilane and vinyltrimethoxysilane in a mass ratio of 1:1.5.

[0033] Furthermore, the preparation method of the aqueous polyurethane solution comprises: mixing polyoxypropylene glycol, polyoxypropylene triol and polyethylene adipate polyol, adding isophorone diisocyanate and a catalyst at 80-90° C., adding composite modified nanopowder after reacting for 1-2 hours, and adding triethylamine for emulsification after 30-60 minutes; adding a chain extender and a crosslinking agent after cooling to room temperature, and reacting again for 1-2 hours to obtain an aqueous polyurethane.

[0034] The beneficial effects of the present invention are:

[0035] The present invention uses polyoxypropylene glycol, polyoxyglycerol, and polyethylene adipate polyol in a ratio of 70-90:80-100:120-200 as composite raw materials, and adds composite modified nano powder, wherein the composite modified nano powder is modified nano calcium carbonate and / or nano titanium dioxide nano powder; and cooperates with the selection of chain extenders, crosslinking agents and catalysts to effectively improve the aging resistance and wear resistance of water-based suede microfiber leather;

[0036] In the present invention, a composite nano-modified material is introduced into the waterborne polyurethane raw material, and the nano-modified material is used as the core to prepare the ultra-fine leather, which effectively improves the wear resistance and aging resistance of the ultra-fine leather. The doping of the composite nano-material does not change the original structure of the polyurethane, but can obviously improve the microscopic morphology and overall uniformity of the composite material, and improve the mechanical properties and wear properties of the composite material.

[0037] The composite nano-modified powders in the present invention are nano-calcium carbonate and nano-titanium dioxide modified by coupling agents, but the difference is that the modified nano-powders are modified in different ways, and the types of coupling agents used are also different. The silane coupling agent in the modified nano-calcium carbonate includes γ-aminopropyltriethoxysilane and γ-glycidyloxypropyltrimethoxysilane in a mass ratio of 1:1, and the silane coupling agent in the modified nano-titanium dioxide includes methyltriethoxysilane and vinyltrimethoxysilane in a mass ratio of 1:1.5. Due to the presence of nanoparticles, the plastic deformation of the material is slowed down, and the transfer film can be made thin and uniform when rubbed, and it is not easy to fall off, thereby slowing down adhesive wear. Based on this, the compounding of the two can effectively and synergistically improve the wear resistance and aging resistance of microfiber leather.

[0038] In the present invention, castor oil and polyoxypropylene glycol are used as a composite cross-linking agent in a mass ratio of 1:1-2, which can significantly improve the bonding strength and the stability of the microfiber leather surface. This also increases the adsorption fastness of the water-based polyurethane to the microfiber leather surface, thereby effectively preventing aging and improving wear resistance. DETAILED DESCRIPTION

[0039] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Example 1

[0041] This embodiment provides a method for preparing an aging-resistant and wear-resistant water-based suede microfiber leather, the steps comprising:

[0042] (1) Preparation of padding solution: Take 70 parts of aqueous polyurethane solution, add 42 parts of water and 8 parts of penetrant TF-107C, and stir evenly;

[0043] The preparation method of the waterborne polyurethane comprises:

[0044] 80 parts of polyoxypropylene glycol (PPG2000), 90 parts of polyoxypropylene glycol (PPG303) and 150 parts of polyethylene adipate polyol (PEA-2000) were mixed, 100 parts of isophorone diisocyanate and 2 parts of dibutyltin dilaurate as a catalyst were added at 85°C, 22 parts of composite modified nanopowder were added after reacting for 1.5 hours, and 12 parts of triethylamine were added for emulsification after 50 minutes; after cooling to room temperature, 17 parts of chain extender 1,4-butanediol and 7 parts of crosslinking agent were added, and the mixture was reacted for another 1.5 hours to obtain waterborne polyurethane;

[0045] The composite nano modified powder includes modified nano calcium carbonate and / or nano titanium dioxide; the weight ratio of the two is 1:2;

[0046] The cross-linking agent includes castor oil and polyoxypropylene glycol in a mass ratio of 1:1.5.

[0047] The preparation method of the modified nano-calcium carbonate comprises: adding 45 ml of anhydrous ethanol and 2.5 g of a silane coupling agent to 42 g of nano-calcium carbonate, stirring, and ultrasonicating for 40 minutes to obtain the modified nano-calcium carbonate; the silane coupling agent is γ-aminopropyltriethoxysilane and γ-glycidyloxypropyltrimethoxysilane in a mass ratio of 1:1;

[0048] The preparation method of the silane coupling agent modified nano titanium dioxide comprises: mixing anhydrous ethanol, deionized water and a silane coupling agent in a weight ratio of (65): (5.5): (15), hydrolyzing for 37 minutes to obtain a mixed solution, mixing nano titanium dioxide and anhydrous ethanol in a weight ratio of 1: (13) and ultrasonically dispersing them, then adding the mixed solution, maintaining at 87° C. for 2.5 hours, filtering, washing and drying to obtain the silane coupling agent modified nano titanium dioxide;

[0049] The mass of the silane coupling agent is 15% of the nano titanium dioxide. The silane coupling agent is a composite silane coupling agent, specifically methyltriethoxysilane and vinyltrimethoxysilane in a mass ratio of 1:1.5;

[0050] (2) Padding: The cut microfibers are immersed in a pre-prepared aqueous polyurethane padding solution. After being fully impregnated, the fabric is passed through a padder and dried at 170°C for 8 minutes. During the padding process, the padding rate is controlled to be 135%; after drying, a water-based suede microfiber leather is obtained.

[0051] Example 2

[0052] This embodiment provides a method for preparing an aging-resistant and wear-resistant water-based suede microfiber leather, the steps comprising:

[0053] (1) Preparation of padding solution: Take 60 parts of aqueous polyurethane solution, add 40 parts of water and 5 parts of penetrant TF-107C, and stir evenly;

[0054] The preparation method of the waterborne polyurethane comprises:

[0055] 70 parts of polyoxypropylene glycol (PPG2000), 80 parts of polyoxypropylene glycol (PPG303) and 120 parts of polyethylene adipate polyol (PEA-2000) were mixed, 80 parts of isophorone diisocyanate and 1 part of dibutyltin dilaurate as a catalyst were added at 80°C, 15 parts of composite modified nanopowder were added after reaction for 1 hour, and 8 parts of triethylamine were added for emulsification after 30 minutes; after cooling to room temperature, 15 parts of chain extender 1,4-butanediol and 6 parts of crosslinking agent were added, and the mixture was reacted for another 1 hour to obtain waterborne polyurethane;

[0056] The composite nano modified powder comprises modified nano calcium carbonate and / or nano titanium dioxide; the weight ratio of the two is 1:1; the cross-linking agent comprises castor oil and polyoxypropylene glycol in a mass ratio of 1:1.

[0057] The preparation method of the modified nano-calcium carbonate comprises: adding 40 ml of anhydrous ethanol and 2 g of a silane coupling agent to 40 g of nano-calcium carbonate, stirring, and ultrasonicating for 30 minutes to obtain the modified nano-calcium carbonate; the silane coupling agent is γ-aminopropyltriethoxysilane and γ-glycidyloxypropyltrimethoxysilane in a mass ratio of 1:1;

[0058] The preparation method of the silane coupling agent modified nano titanium dioxide comprises: mixing anhydrous ethanol, deionized water and a silane coupling agent in a weight ratio of (60): (5): (12), hydrolyzing for 30 minutes to obtain a mixed solution, mixing nano titanium dioxide and anhydrous ethanol in a weight ratio of 1: (12) and ultrasonically dispersing them, then adding the mixed solution, maintaining at 85° C. for 2 hours, filtering, washing and drying to obtain the silane coupling agent modified nano titanium dioxide;

[0059] The mass of the silane coupling agent is 10% of the nano titanium dioxide. The silane coupling agent is a composite silane coupling agent, specifically methyltriethoxysilane and vinyltrimethoxysilane in a mass ratio of 1:1.5;

[0060] (2) Padding: The cut microfibers are immersed in the prepared aqueous polyurethane padding solution. After being fully impregnated, the fabric is passed through a padder and dried at 160°C for 6 minutes. During the padding process, the padding rate is controlled to be 120%; after drying, the aqueous suede microfiber leather is obtained.

[0061] Example 3

[0062] This embodiment provides a method for preparing an aging-resistant and wear-resistant water-based suede microfiber leather, the steps comprising:

[0063] (1) Preparation of padding solution: Take 80 parts of aqueous polyurethane solution, add 45 parts of water and 12 parts of penetrant TF-107C, and stir evenly;

[0064] The preparation method of the waterborne polyurethane comprises:

[0065] 90 parts of polyoxypropylene glycol (PPG2000), 100 parts of polyoxypropylene glycol (PPG303) and 200 parts of polyethylene adipate polyol (PEA-2000) were mixed, 110 parts of isophorone diisocyanate and 3 parts of dibutyltin dilaurate as a catalyst were added at 90°C, 30 parts of composite modified nanopowder were added after reacting for 2 hours, and 15 parts of triethylamine were added for emulsification after 60 minutes; after cooling to room temperature, 20 parts of chain extender 1,4-butanediol and 8 parts of crosslinking agent were added, and the mixture was reacted for another 2 hours to obtain waterborne polyurethane;

[0066] The composite nano modified powder comprises modified nano calcium carbonate and / or nano titanium dioxide; the weight ratio of the two is 1:3; the cross-linking agent comprises castor oil and polyoxypropylene glycol in a mass ratio of 1:2.

[0067] The preparation method of the modified nano-calcium carbonate comprises: adding 50 ml of anhydrous ethanol and 3 g of a silane coupling agent to 45 g of nano-calcium carbonate, stirring, and ultrasonicating for 60 minutes to obtain the modified nano-calcium carbonate; the silane coupling agent is γ-aminopropyltriethoxysilane and γ-glycidyloxypropyltrimethoxysilane in a mass ratio of 1:1;

[0068] The preparation method of the silane coupling agent modified nano titanium dioxide comprises: mixing anhydrous ethanol, deionized water and a silane coupling agent in a weight ratio of (70): (6): (18), hydrolyzing for 45 minutes to obtain a mixed solution, mixing nano titanium dioxide and anhydrous ethanol in a weight ratio of 1: (15), ultrasonically dispersing, then adding the mixed solution, maintaining at 90° C. for 3 hours, filtering, washing and drying to obtain the silane coupling agent modified nano titanium dioxide;

[0069] The mass of the silane coupling agent is 20% of the nano titanium dioxide. The silane coupling agent is a composite silane coupling agent, specifically methyltriethoxysilane and vinyltrimethoxysilane in a mass ratio of 1:1.5;

[0070] (2) Padding: The cut microfibers are immersed in the prepared aqueous polyurethane padding solution. After being fully impregnated, the fabric is passed through a padder and dried at 180°C for 10 minutes. During the padding process, the padding rate is controlled to be 150%; after drying, the aqueous suede microfiber leather is obtained.

[0071] Example 4

[0072] This embodiment provides a method for preparing an aging-resistant and wear-resistant water-based suede microfiber leather, the steps comprising:

[0073] (1) Preparation of padding solution: Take 60 parts of aqueous polyurethane solution, add 45 parts of water and 12 parts of penetrant TF-107C, and stir evenly;

[0074] The preparation method of the waterborne polyurethane comprises:

[0075] 90 parts of polyoxypropylene glycol (PPG2000), 80 parts of polyoxypropylene glycol (PPG303) and 120 parts of polyethylene adipate polyol (PEA-2000) were mixed, 80 parts of isophorone diisocyanate and 3 parts of dibutyltin dilaurate as a catalyst were added at 80°C, 30 parts of composite modified nanopowder were added after reacting for 2 hours, and 15 parts of triethylamine were added for emulsification after 30 minutes; after cooling to room temperature, 20 parts of chain extender 1,4-butanediol and 8 parts of crosslinking agent were added, and the mixture was reacted for another 2 hours to obtain waterborne polyurethane;

[0076] The composite nano modified powder comprises modified nano calcium carbonate and / or nano titanium dioxide; the weight ratio of the two is 1:1; the cross-linking agent comprises castor oil and polyoxypropylene glycol in a mass ratio of 1:2.

[0077] The preparation method of the modified nano-calcium carbonate comprises: adding 50 ml of anhydrous ethanol and 3 g of a silane coupling agent to 45 g of nano-calcium carbonate, stirring, and ultrasonicating for 60 minutes to obtain the modified nano-calcium carbonate; the silane coupling agent is γ-aminopropyltriethoxysilane and γ-glycidyloxypropyltrimethoxysilane in a mass ratio of 1:1;

[0078] The preparation method of the silane coupling agent modified nano titanium dioxide comprises: mixing anhydrous ethanol, deionized water and a silane coupling agent in a weight ratio of (60): (5): (18), hydrolyzing for 45 minutes to obtain a mixed solution, mixing nano titanium dioxide and anhydrous ethanol in a weight ratio of 1: (15), ultrasonically dispersing, then adding the mixed solution, maintaining at 90° C. for 3 hours, filtering, washing and drying to obtain the silane coupling agent modified nano titanium dioxide;

[0079] The mass of the silane coupling agent is 20% of the nano titanium dioxide. The silane coupling agent is a composite silane coupling agent, specifically methyltriethoxysilane and vinyltrimethoxysilane in a mass ratio of 1:1.5;

[0080] (2) Padding: The cut microfibers are immersed in the prepared aqueous polyurethane padding solution. After being fully impregnated, the fabric is passed through a padder and dried at 160°C for 6 minutes. During the padding process, the padding rate is controlled to be 120%; after drying, the aqueous suede microfiber leather is obtained.

[0081] Comparative Example 1

[0082] The difference from Example 1 is that the composite modified nano powder is not used in Comparative Example 1, but is replaced by modified nano calcium carbonate of equal mass.

[0083] Comparative Example 2

[0084] Different from Example 1, in Comparative Example 2, no composite modified nano powder was used, but instead, an equal mass of modified nano titanium dioxide was used.

[0085] Comparative Example 3

[0086] Different from Example 1, in Comparative Example 3, polyethylene adipate polyol was not used, but was replaced by polyoxypropylene glycol and polyoxypropylene glycol in equal weight and proportion.

[0087] Comparative Example 4

[0088] Different from Example 1, in Comparative Example 4, polyoxypropylene glycol and polyoxyglycerol were not used, but were replaced by polyethylene adipate polyol of equal mass.

[0089] Comparative Example 5

[0090] Different from Example 1, the nano powder added in Comparative Example 5 was not modified, but replaced with nano powder of equal proportion and mass.

[0091] Comparative Example 6

[0092] Different from Example 1, Comparative Example 6 only contains modified nano-calcium carbonate, wherein the silane coupling agent is γ-aminopropyltriethoxysilane.

[0093] Comparative Example 7

[0094] Different from Example 1, Comparative Example 7 only contains modified nano-titanium dioxide, wherein the silane coupling agent is vinyltrimethoxysilane.

[0095] Comparative Example 8

[0096] Different from Example 1, in Comparative Example 8, no composite modified nano powder was added.

[0097] The following performance tests were performed on the water-based suede microfiber leathers prepared in Examples 1 to 4 and Comparative Examples 1 to 8:

[0098] (1) The abrasion was tested by Martindale test for 35,000 times according to GB / T21196.2-2007. During the test, the suede layer of the water-based suede microfiber leather was used as the friction surface.

[0099] (2) Abrasion resistance test: Abrasion resistance is tested in accordance with GB / T 2726-2005 "Determination of abrasion resistance of leather by physical and mechanical tests" (test times: 500 revolutions); (CS-R, 1000G)

[0100] (3) Aging resistance test: After the sample is irradiated with ultraviolet light (40W) for 2000h, the elongation retention rate is tested, where the elongation retention rate = elongation after irradiation / elongation before irradiation*100%;

[0101] The test results are shown in Table 1 below:

[0102] Table 1

[0103]

[0104] Finally, it should be noted that the above embodiments are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. All technical solutions and improvements that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing aging-resistant and wear-resistant water-based suede microfiber leather, characterized in that the steps include: Preparation of padding solution: Add water and penetrant to the aqueous polyurethane solution and stir evenly; Wherein, the raw materials of the waterborne polyurethane include: Polyoxypropylene glycol, polyoxypropylene glycol, polyethylene adipate polyol, isophorone diisocyanate, chain extender, crosslinking agent, catalyst and composite modified nano powder; Padding: Immerse the cut microfibers in the prepared water-based polyurethane padding solution. After fully impregnated, pass the fabric through a padder and dry it at 160-180°C for 6-10 minutes. The cross-linking agent includes castor oil and polyoxyglycerol in a mass ratio of 1:1-2, the chain extender includes 1,4-butanediol and / or 1,3-propylene glycol, and the catalyst includes dibutyltin dilaurate; The raw materials of the waterborne polyurethane include: 70-90 parts of polyoxypropylene glycol, 80-100 parts of polyoxypropylene glycol, 120-200 parts of polyethylene adipate polyol, 80-110 parts of isophorone diisocyanate, Chain extender 15-20 parts, 6-8 parts of cross-linking agent, 1-3 parts of catalyst, 15-30 parts of composite modified nano powder; The composite modified nano powder includes modified nano calcium carbonate and nano titanium dioxide; The preparation method of the modified nano calcium carbonate comprises: adding anhydrous ethanol and a silane coupling agent to the nano calcium carbonate, stirring, and ultrasonicating for 30-60 minutes to obtain the modified nano calcium carbonate; The silane coupling agent in the preparation process of modified nano-calcium carbonate includes γ-aminopropyltriethoxysilane and γ-glycidyloxypropyltrimethoxysilane in a mass ratio of 1:1; The preparation method of the modified nano titanium dioxide comprises: mixing anhydrous ethanol, deionized water and a silane coupling agent, hydrolyzing for 30-45 minutes to obtain a mixed solution, mixing the nano titanium dioxide and the anhydrous ethanol for ultrasonic dispersion, then adding the mixed solution, maintaining at 85-90° C. for 2-3 hours, filtering, washing and drying to obtain the silane coupling agent modified nano titanium dioxide; The silane coupling agent used in the preparation process of modified nano-titanium dioxide includes methyltriethoxysilane and vinyltrimethoxysilane in a mass ratio of 1:1.

5.

2. The method for preparing an aging-resistant and wear-resistant water-based suede microfiber leather according to claim 1, characterized in that: The weight ratio of anhydrous ethanol, deionized water and silane coupling agent is (60-70): (5-6): (12-18); the weight ratio of nano titanium dioxide and anhydrous ethanol is 1: (12-15); the mass of the silane coupling agent is 10-20% of the nano titanium dioxide.

3. The method for preparing an aging-resistant and wear-resistant water-based suede microfiber leather according to claim 1, characterized in that: The preparation method of the waterborne polyurethane comprises: mixing polyoxypropylene glycol, polyoxyglycerol and polyethylene adipate polyol, adding isophorone diisocyanate and a catalyst under the condition of 80-90° C., reacting for 1-2 hours, adding composite modified nano powder, adding triethylamine for emulsification after 30-60 minutes; adding a chain extender and a crosslinking agent after cooling to room temperature, and reacting again for 1-2 hours to obtain the waterborne polyurethane.