A method for manufacturing DM paper
By using mixed pulp of bleached sulfate coniferous chemical pulp, broadleaf chemical pulp and poplar mechanical pulp, combined with new coating formula and calendering treatment, the problem of insufficient printing gloss of existing DM single paper is solved, and the printing of existing DM is achieved. Quality improvement and cost control of high-end products.
Patent Information
- Application Number
- CN202311046300.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-18
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-08-18
AI Technical Summary
The printing gloss and surface strength of existing DM single papers are insufficient, making it difficult to meet the usage requirements of high-end customers.
Using mixed pulp of bleached sulfate coniferous pulp, bleached sulfate broadleaf wood chemical pulp and alkaline hydrogen peroxide mechanical pulp, and developing a new coating formula, including three The carboxylic acid copolymer was subjected to double-side coating and post-drying calendering.
It significantly improves the printing gloss and surface strength of DM single paper, meets the needs of high-end customers, improves product quality and reduces costs.
Smart Images

Figure BDA0004402600360000061 
Figure BDA0004402600360000111 
Figure BDA0004402600360000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of papermaking, and in particular relates to a method for manufacturing DM single paper. Background Art
[0002] DM is a form of advertising leaflet. DM is the abbreviation of direct mail advertising in English. It is to send the advertising leaflet to consumers, their homes or company locations by mailing or giving it as a gift. DM broadly includes advertising leaflets, such as flyers distributed on the streets, in shopping malls and supermarkets, paper coupons from merchants, etc.
[0003] DM single base paper generally has good gloss, high opacity, uniform thickness, good evenness, low roughness, high surface strength, etc. In the domestic general coated advertising paper manufacturing, the fiber raw material is usually full chemical pulp, and the paper weight is 48-64g / m 2 , mainly using heavy calcium, porcelain clay, and adhesive (styrene butadiene) and other coating compositions for coating and other production processes. However, the performance of paper printing gloss strength and other properties of existing DM single paper in China needs to be improved. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a method for manufacturing DM single paper. The DM single paper developed by the present invention has a fine surface and excellent printing gloss effect.
[0005] The present invention provides a method for manufacturing DM paper, comprising the following steps:
[0006] Using bleached kraft softwood chemical pulp, bleached kraft hardwood chemical pulp and alkaline hydrogen peroxide poplar mechanical pulp as raw materials, the process includes pulping, pulping and auxiliary material addition, wet paper sheet forming, pre-drying, coating and sizing, and post-drying to obtain DM single paper;
[0007] The bleached kraft coniferous wood chemical pulp is mixed with industrial hemp, and the mass ratio of the bleached kraft coniferous wood chemical pulp, the bleached kraft broadleaf wood chemical pulp and the alkaline hydrogen peroxide poplar wood mechanical pulp is 25-30%: 20-25%: 45-50%;
[0008] The coating formula used for coating and sizing includes, by weight: 10-20 parts of Brazilian clay, 5-10 parts of aluminum oxide, 15-20 parts of talcum powder, 50-70 parts of coating-grade heavy calcium carbonate, 10-15 parts of styrene-butadiene latex and 0.1-0.2 parts of tricarboxylic acid copolymer.
[0009] Preferably, after the respective beating, the freeness of bleached kraft coniferous wood chemical pulp is 275-325 mL; the freeness of bleached kraft hardwood chemical pulp is 285-335 mL; and the freeness of alkaline hydrogen peroxide poplar mechanical pulp is 200-230 mL.
[0010] Preferably, 0.4-0.8 kg / t of sodium carboxymethyl cellulose is added to the bleached kraft coniferous wood chemical pulp and the bleached kraft hardwood chemical pulp during pulping.
[0011] Preferably, the components added as auxiliary materials include fillers, cationic starch, polyacrylamide, bentonite and organic particles.
[0012] Preferably, in the auxiliary materials, the weight ratio of filler is 8-10%; the weight ratio of cationic starch is 0.7-1.1%; and the weight ratio of bentonite is 0.15-0.35%.
[0013] Preferably, the coating formula further comprises a defoamer; and the solid content of the coating is 65-67%.
[0014] Preferably, the coating is a double-sided coating process, and the total coating amount is 15-19 g / m 2 .
[0015] Preferably, during the double-sided coating process, the coating amount on the front side is greater than the coating amount on the back side.
[0016] Preferably, the post-drying further includes calendering, and the calendering adopts an 8-roller 7-nip pressure mode with a pressure of 200-250 kN / m.
[0017] Preferably, the moisture content of the paper sheet obtained by the post-drying is 6-9%; and the calendering temperature is 180-250°C.
[0018] Preferably, the DM single paper has a basis weight of 48-64 g / m 2 , the smoothness of the front side of the paper is greater than 700s, the roughness of the front side is less than 1.7μm, and the glossiness of the front side is greater than 40%.
[0019] Compared with the prior art, the method of the present invention is to promote the high-end development of DM single products. First, a mixture of coniferous chemical pulp, hardwood chemical pulp and poplar chemical mechanical pulp is used for production. A small amount of industrial hemp is added to the coniferous chemical pulp, which is conducive to the fineness of the paper surface. In addition, a new coating formula is developed accordingly, including: increasing the amount of talcum powder to replace part of the porcelain clay; using tricarboxylic acid copolymer to improve the rheological properties of the coating; adding 5-10 parts by mass of aluminum oxide, etc., to improve the gloss of the printing. The experimental results show that the DM paper produced has a basis weight of 56g / m 2, moisture content is 4.5-5.5%, whiteness ISO is greater than 75%, front smoothness is greater than 700s, front roughness is less than 1.7μm, front gloss is greater than 40%, longitudinal tear length is greater than 4500m, and transverse folding endurance is greater than 10 times. The DM single paper surface gloss, printing gloss, and surface strength effects described in the embodiment of the present invention are significantly improved, with high quality and low cost, which is conducive to application and has great significance for expanding the coating product market and increasing product profit margins. DETAILED DESCRIPTION
[0020] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is described in detail below in conjunction with specific embodiments. The description in this section is only exemplary and explanatory and should not have any limiting effect on the scope of protection of the present invention.
[0021] The present invention provides a method for manufacturing DM paper, comprising the following steps:
[0022] Using bleached kraft softwood chemical pulp, bleached kraft hardwood chemical pulp and alkaline hydrogen peroxide poplar mechanical pulp as raw materials, the process includes pulping, pulping and auxiliary material addition, wet paper sheet forming, pre-drying, coating and sizing, and post-drying to obtain DM single paper;
[0023] The bleached kraft coniferous wood chemical pulp is mixed with industrial hemp, and the mass ratio of the bleached kraft coniferous wood chemical pulp, the bleached kraft broadleaf wood chemical pulp and the alkaline hydrogen peroxide poplar wood mechanical pulp is 25-30%: 20-25%: 45-50%;
[0024] The coating formula used for coating and sizing includes, by weight: 10-20 parts of Brazilian clay, 5-10 parts of aluminum oxide, 15-20 parts of talcum powder, 50-70 parts of coating-grade heavy calcium carbonate, 10-15 parts of styrene-butadiene latex and 0.1-0.2 parts of tricarboxylic acid copolymer.
[0025] The DM single paper produced by the process of the present invention has a fine surface and excellent printing glossiness and other effects, which can fully meet the high-end usage requirements of customers and is of great significance for enterprises to optimize product structure and improve company profitability.
[0026] In order to make the surface of paper fine and smooth, the embodiment of the present invention adopts a mixed pulp of coniferous chemical pulp, hardwood chemical pulp and poplar chemical mechanical pulp for production, wherein a small amount of industrial hemp is mixed in the coniferous chemical pulp, such as adding industrial hemp with a mass ratio of 5-10%. In the embodiment of the present invention, the pulp is coniferous chemical pulp, hardwood chemical pulp and poplar chemical mechanical pulp, corresponding to bleached sulfate coniferous chemical pulp (NBKP, mixed with a small amount of industrial hemp, referred to as coniferous pulp), bleached sulfate hardwood chemical pulp (LBKP, referred to as hardwood pulp), alkaline hydrogen peroxide bleached poplar mechanical pulp (APMP), commercially available fiber raw materials can be used, and pulping can also be done by oneself. In addition, the mass ratio of the pulp is coniferous pulp: hardwood pulp: poplar chemical mechanical pulp = 25-30%: 20-25%: 45-50%.
[0027] The specific embodiment of the present invention is to pre-treat and pulp the wood chip raw materials: after screening, dust removal and cleaning, coniferous wood chips, industrial hemp and broadleaf wood chips are mixed in a silo at a ratio of 25-30% (including 5-10% industrial hemp): 20-25% and then sent to a cooking pot, wherein a small amount of industrial hemp is first removed from the hemp skin and sliced and then mixed into the coniferous wood chips, and the pulping is carried out by the kraft method, oxygen delignification, hydrogen peroxide bleaching and cleaning, and the pulping requirements are: whiteness of 27-31% ISO; Kappa number of 36-42. The cleaned pulp is sent to the pulp storage tower and sent to the pulping system with clean water. The poplar raw material is prepared by the PRC-APMP (P represents pre-refining pretreatment, represents disc grinding to promote the chemical action of pulp, and APMP represents alkaline hydrogen peroxide mechanical pulp) pulping process to make poplar chemical mechanical pulp with a whiteness of 76% ISO and a beating degree of 54-58°SR.
[0028] In the embodiment of the present invention, the prepared pulp can be pulped separately, and the pulping method is preferably three mills in series. In the embodiment of the present invention, the concentration of the pulping is preferably 3.6-4%; the pulping is mainly based on decomposition and brooming, and the principle requires less cutting. Preferably, 0.4-0.8kg / t of sodium carboxymethyl cellulose (CMC) is added to NBKP and LBKP pulping to enhance fiber fibrillation and brooming. Specifically, the pulp freeness requirements after pulping are coniferous pulp (275-325ml), broadleaf pulp (285-335ml), and poplar chemical mechanical pulp (200-230ml).
[0029] The above three slurries are prepared in proportion, and auxiliary materials are added; the components of the auxiliary materials include fillers, cationic starch, polyacrylamide, bentonite and organic particles. Among the auxiliary materials, the weight ratio of fillers relative to the absolute dry pulp dosage is preferably 8-10%; the weight ratio of cationic starch is preferably 0.7-1.1%; the preferred bentonite weight ratio is 0.15-0.35%; and the retention aid polyacrylamide is preferably 300-500ppm, and the type is preferably cationic PAM; the organic particles can be modified diatomaceous earth, with a weight ratio of 200-400ppm. The embodiment of the present invention is composed of commercially available cationic starch and other auxiliary materials for papermaking; wherein the performance indicators of cationic PAM include: molecular weight of 5 million-10 million, cationization degree of 10-20%; the performance indicators of modified diatomaceous earth include: bulk density of 0.34-0.65g / cm 3 , pH value 6.0-8.0, specific surface area 40-65m 2 / g.
[0030] In a preferred embodiment of the present invention, the added filler can be a light calcium carbonate (grade 60) filler, which is sent to a first-stage four-stage conical slag remover for purification and slag removal through a slurry pump, and then enters a degassing tank for degassing treatment; thereafter, it enters a pressure screen for screening treatment (cationic PAM dosage 0.4-0.6 kg / ton of paper, cationic starch 10 kg / ton of paper, both added at the pressure screen inlet, modified diatomaceous earth 2.2-2.8 kg / ton of paper, added at the pressure screen outlet).
[0031] In the embodiment of the present invention, the slurry after the auxiliary material is added is sent to the headbox to be screened, and the screen flow rate is adjusted to control the scanning paper sheet basis weight before sizing to be 42-47 g / m 2 The wet paper leaves the screen and enters the pressing section, preferably a five-roller three-nip composite pressing. After pressing to a dryness of ≥39%, the paper enters the pre-drying section; the surface temperature of the drying cylinder is preferably controlled at 90-130°C, and the paper is dried to a dryness of ≥95%.
[0032] Next, the paper sheet is fed into a coating machine to be coated on the front and back sides of the paper sheet. The coating and sizing process is a double-sided coating process with a total coating amount of 15 to 19 g / m 2 Specifically, the components of the front coating formula are measured by weight: 10-20 parts of Brazilian porcelain clay, 5-10 parts of aluminum oxide, 15-20 parts of talc, 50-70 parts of coating-grade heavy calcium carbonate (95-grade heavy calcium carbonate), 10-15 parts of styrene-butadiene latex, 0.1-0.2 parts of tricarboxylic acid copolymer, and other trace additives in appropriate amounts; the coating solid content is preferably 65-67%, and the defoamer is appropriate; the front coating amount is preferably 8-10 g / m 2 ;
[0033] The components of the reverse coating formula are calculated by weight: 10-20 parts of Brazilian porcelain clay, 5-10 parts of aluminum oxide, 15-20 parts of talc, 50-70 parts of coating grade heavy calcium carbonate (grade 95), 10-15 parts of styrene-butadiene latex, 0.1-0.2 parts of tricarboxylic acid copolymer, and other trace additives in appropriate amounts. The solid content of the coating is 65-67%, and the defoaming agent is in appropriate amounts. The reverse coating amount is preferably 7g / m 2 In the double-sided coating process, the coating amount on the front side is greater than that on the back side. The embodiment of the present invention can significantly reduce production costs by using different coating amounts on the front and back sides of the base paper, which has a significant cost advantage.
[0034] The embodiment of the present invention adopts the above-mentioned new coating formula independently developed, wherein china clay can effectively improve the glossiness, heavy calcium can effectively reduce the cost, and latex mainly improves the bonding strength of the coating. The present invention increases the amount of talcum powder and replaces a part of china clay. In order to effectively improve the rheological properties of the coating, a tricarboxylic acid copolymer (whose molecular weight can be 5000-8000 and room temperature viscosity is 100-400mpa·s) is used. At the same time, in order to improve the printing glossiness, etc., the present invention adds 5-10 parts by mass of aluminum oxide for coordination.
[0035] The coating is prepared by taking the pigment (including china clay, aluminum oxide, talcum powder, heavy calcium carbonate) as 100%. The mass percentage of other components relative to the pigment is the number of other components, wherein china clay, aluminum oxide, talcum powder, heavy calcium carbonate are prepared with solid contents of 68-72%, 55-60%, 64-68%, 73-77% respectively (mixed with water), and then mixed in the above order under high-speed shearing (such as 2000r / min), and then mixed in the order of styrene-butadiene latex, tricarboxylic acid copolymer, and trace additives, and mixed evenly under high-speed shearing.
[0036] The components in the coating formula of the embodiment of the present invention can be corresponding commercially available products; wherein, the solid content of styrene-butadiene latex can be 48-52%, the pH value is 5.0-7.0, and the room temperature viscosity is less than 300mPa·s. Other trace additives are calcium stearate lubricant and / or polyamide polyurea water repellent; the main components of the defoamer include polyether, higher alcohol, mineral oil and other active ingredients, which play a role in eliminating foam. The components of the coating system are combined with other additives and defoamers to form the above-mentioned certain solid content, and there is no special restriction on other additives and defoamers.
[0037] Specific coating conditions include: pressure in the nip: transmission side / operation side: 17-24 / 17-24 kN / m, pressure on the metering rod: upper roller / lower roller: 0.7-1.4 / 0.7-1.4 bar, coating amount: 15-19 g / m 2 ;The paper tension setting value is 330N / m.
[0038] The present invention example adds tricarboxylic acid copolymer, aluminum oxide, and talcum powder to conduct comparative experiments, and the performance comparison results are shown in the following table. In the comparative experiment, the coating formula is: 10-20 parts of Brazilian porcelain clay, 50-70 parts of coating grade heavy calcium carbonate (95 grade heavy calcium carbonate), and 10-15 parts of styrene-butadiene latex.
[0039] Table 1 Comparison of coating formulations in the embodiments of the present invention
[0040]
[0041] In the embodiment of the present invention, after adding the tricarboxylic acid copolymer, the experiment obtained the high shear viscosity and low shear viscosity data, which proved that the rheology and running performance of the coating were improved. After adding aluminum oxide, the glossiness of the paper surface and the glossiness of the printing were obviously improved. After adding talcum powder, the experiment showed that the glossiness of the paper surface, the glossiness of the printing, and the surface strength were all significantly improved.
[0042] After coating and sizing, the coated paper sheet obtained in the embodiment of the present invention enters the post-drying treatment, and the dryness of the paper sheet out of the post-drying section is ≥93%. In addition, the paper sheet produced from the post-drying section preferably enters the calendering area to perform calendering treatment on the paper sheet. The calender used can select an 8-roller 7-pressure zone pressure mode, and the pressure is preferably 200-250 kN / m, more preferably 210-240 kN / m; the calendering temperature of the three hot rollers is preferably 180°C to 250°C, and more preferably 185-245°C; the moisture content of the paper sheet before calendering is 6-9%. After calendering, the paper is rolled up to obtain a DM single paper product.
[0043] The embodiment of the present invention adopts a conventional paper machine for production, and other parameters of the paper machine include: a wire speed of 1200-1400 m / min, a pulp-to-wire speed ratio of 1.045-1.047, a first pressing line pressure of 160-170 kN / m, a second pressing line pressure of 700 kN / m, a lip plate opening of 9-10 mm, a hard calendering line pressure of 22-24 kN / m, and a paper tension at hard calendering: 240-250 N / m.
[0044] The DM paper produced by the present invention has a basis weight of 48-64 g / m 2 , specifically 56g / m 2 The moisture content of the paper is 4.5-5.5%, the whiteness ISO is greater than 75%, such as 82.0-84.0% ISO, the front smoothness is greater than 700s, the front roughness is less than 1.7μm, the front gloss is greater than or equal to 40%, such as 41-50%, the longitudinal tear length is greater than 4500m, and the transverse folding endurance is greater than 10 times.
[0045] In order to better understand the technical content of the present invention, the following specific examples are provided to further illustrate the present invention. In the following examples, unless otherwise specified, all are mass ratios; the raw materials used are commercially available and conventional equipment is used. Among them, the performance indicators of cationic PAM are molecular weight 5-10 million, cationization degree 10-20%; the performance indicators of modified diatomaceous earth include: bulk density 0.34-0.65g / cm 3 , pH value 6.0-8.0, specific surface area 40-65m2 / g. Types of defoamers include polyether, higher alcohol, mineral oil, etc. Styrene-butadiene latex solid content 48-52%, pH value 5.0-7.0, viscosity <300mPa.s.
[0046] Embodiment 1:
[0047] Raw material pretreatment and pulping: After screening, dust removal and cleaning of coniferous wood chips, industrial hemp and broadleaf wood chips, they are mixed evenly in a silo at a ratio of 25% (including 5% industrial hemp): 20% and then sent to the cooking pot. A small amount of industrial hemp is first removed from the hemp skin and sliced before being mixed into the coniferous wood chips. The pulping is done by the sulfate method, oxygen delignification, hydrogen peroxide bleaching and cleaning. The pulping requirements are: whiteness 27-31% ISO; Kappa number 36-42. The cleaned pulp is sent to the pulp storage tower and sent to the pulping system with clean water. The poplar raw material is prepared and the PRC-APMP pulping process is used to make poplar chemical mechanical pulp with a whiteness of 76% ISO and a beating degree of 54-58°SR.
[0048] Beating: Beat the prepared pulp in three mills in series. Beating concentration: 3.6-4%. Beating is mainly for decomposition and brooming. In principle, less cutting is required. NBKP and LBKP are beaten with 0.4-0.8kg / t of sodium carboxymethyl cellulose (CMC). The freeness of the pulp after beating is 275-325ml for coniferous pulp, 285-335ml for broadleaf pulp, and 200-230ml for poplar chemical mechanical pulp.
[0049] The three pulps are mixed in the ratio of 25%:30%:45%; then 10% filler-grade light calcium carbonate (grade 60) filler is added, and sent to the first-stage four-stage conical slag remover for purification and slag removal through a slurry pump, and then enter the degassing tank for degassing; then enter the pressure screen for screening (cationic PAM dosage 0.5kg / ton paper, cationic starch 10kg / ton paper, both added at the pressure screen inlet, modified diatomaceous earth 2.2kg / ton paper, added at the pressure screen outlet).
[0050] Then the mixed slurry is sent to the headbox to be screened, and the screen flow is adjusted to control the scanned paper weight at 45g / m 2Around; after the wet paper leaves the screen section, it enters the pressing section for five-roller three-pressure zone composite pressing. After being pressed to a dryness ≥ 39%, it enters the pre-drying section; the surface temperature of the drying cylinder is controlled at 90-130°C to dry the paper until the dryness of the paper is ≥ 95%.
[0051] Next, the paper sheet enters the coating machine for surface treatment on the front and back sides: the components of the front coating formula are by weight: 10 parts of Brazilian clay, 5 parts of aluminum oxide, 15 parts of talcum powder, 50 parts of coating grade heavy calcium carbonate (grade 95), 10 parts of styrene-butadiene latex, 0.1 parts of tricarboxylic acid copolymer (molecular weight 5000-8000, viscosity 100-400mpas), other trace additives in appropriate amounts, coating solid content 65-67%, defoamer in appropriate amounts; front coating amount 8g / m 2 ; The components of the reverse coating formula are by weight: 10 parts of Brazilian porcelain clay, 5 parts of aluminum oxide, 15 parts of talc, 50 parts of coating grade heavy calcium carbonate (grade 95), 10 parts of styrene-butadiene latex, 0.1 parts of tricarboxylic acid copolymer, appropriate amount of other trace additives, coating solid content 65-67%, appropriate amount of defoamer; reverse coating amount 7g / m 2 .
[0052] Coating conditions: Nip pressure: drive side / operation side: 17-24 / 17-24 kN / m, metering rod pressure: upper roller / lower roller: 0.7-1.4 / 0.7-1.4 bar, coating amount: 15 g / m 2 ;The paper tension setting value is 330N / m.
[0053] The coated paper sheets enter the post-drying process, and the dryness of the paper sheets out of the post-drying section is ≥93%; the paper sheets produced from the post-drying section enter the calendering area for calendering. The calender uses an 8-roller 7-nip pressure mode with a pressure of 210-245 kN / m; the calendering temperature of the 3 hot rollers is 185℃-245℃; after calendering, the paper is rolled up to obtain a basis weight of 56g / m 2 , whiteness 82.0~84.0% ISO, front gloss 42% DM single paper, can fully meet the high-end usage requirements of customers.
[0054] Other parameters of the paper machine: wire speed 1300m / min, pulp-to-wire speed ratio 1.046, first calendering pressure: 165kN / m, second calendering pressure: 700kN / m, lip opening: 9.5mm, hard calendering line pressure: 23kN / m, paper tension at hard calendering: 245N / m.
[0055] Embodiment 2:
[0056] Raw material pretreatment and pulping: After screening, dust removal and cleaning, coniferous wood chips, industrial hemp and broadleaf wood chips are mixed in a silo at a ratio of 28% (including 8% industrial hemp): 22% and then sent to the cooking pot. A small amount of industrial hemp is first removed from the hemp skin and sliced before being mixed into the coniferous wood chips. The pulping is made by the sulfate method, oxygen delignification, hydrogen peroxide bleaching and cleaning. The pulping requirements are: whiteness 27-31% ISO; Kappa number 36-42. The cleaned pulp is sent to the pulp storage tower and sent to the pulping system with clean water. The poplar raw material is prepared and the PRC-APMP pulping process is used to make poplar chemical mechanical pulp with a whiteness of 76% ISO and a beating degree of 54-58°SR.
[0057] Beating: Beat the prepared pulp in three mills in series. Beating concentration: 3.6-4%. Beating is mainly for decomposition and brooming. In principle, less cutting is required. NBKP and LBKP are beaten with 0.4-0.8kg / t of sodium carboxymethyl cellulose (CMC). The freeness of the pulp after beating is 275-325ml for coniferous pulp, 285-335ml for broadleaf pulp, and 200-230ml for poplar chemical mechanical pulp.
[0058] The three pulps are mixed in the ratio of 30%:30%:40%; then 12% filler-grade light calcium carbonate (grade 60) filler is added, and sent to a first-stage four-stage conical slag remover for purification and slag removal through a slurry pump, and then enter the degassing tank for degassing; then enter the pressure screen for screening (cationic PAM dosage 0.4kg / ton paper, cationic starch 10kg / ton paper, both added at the pressure screen inlet, modified diatomaceous earth 2.2kg / ton paper, added at the pressure screen outlet).
[0059] Then the mixed slurry is sent to the headbox to be screened, and the screen flow is adjusted to control the scanned paper weight at 45g / m 2 Around; after the wet paper leaves the screen section, it enters the pressing section for five-roller three-pressure zone composite pressing. After being pressed to a dryness ≥ 39%, it enters the pre-drying section; the surface temperature of the drying cylinder is controlled at 90-130°C to dry the paper until the dryness of the paper is ≥ 95%.
[0060] Next, the paper sheet enters the coating machine for surface treatment on the front and back sides: the components of the front coating formula are by weight: 15 parts of Brazilian clay, 8 parts of aluminum oxide, 18 parts of talcum powder, 60 parts of coating grade heavy calcium carbonate (grade 95), 12 parts of styrene-butadiene latex, 0.15 parts of tricarboxylic acid copolymer (molecular weight 5000-8000, viscosity 100-400mpas), other trace additives in appropriate amounts, coating solid content 65-67%, defoamer in appropriate amounts; front coating amount 8g / m 2; The components of the reverse coating formula are by weight: 15 parts of Brazilian porcelain clay, 8 parts of aluminum oxide, 18 parts of talc, 60 parts of coating grade heavy calcium carbonate (grade 95), 12 parts of styrene-butadiene latex, 0.15 parts of tricarboxylic acid copolymer, appropriate amount of other trace additives, coating solid content 65-67%, appropriate amount of defoamer; reverse coating amount 7g / m 2 The coating conditions are the same as in Example 1.
[0061] The coated paper sheets enter the post-drying process, and the dryness of the paper sheets out of the post-drying section is ≥93%; the paper sheets produced from the post-drying section enter the calendering area for calendering. The calender uses an 8-roller 7-nip pressure mode with a pressure of 210-245 kN / m; the calendering temperature of the 3 hot rollers is 185℃-245℃; after calendering, the paper is rolled up to obtain a basis weight of 56g / m 2 , whiteness 82.0~84.0% ISO, front gloss 42% DM single paper, can fully meet the high-end usage requirements of customers.
[0062] The other parameters of the paper machine are the same as those in Example 1.
[0063] Embodiment 3:
[0064] Raw material pretreatment and pulping: After screening, dust removal and cleaning of coniferous wood chips, industrial hemp and broadleaf wood chips, they are mixed evenly in the silo at a ratio of 30% (including 10% industrial hemp): 25% and then sent to the cooking pot. A small amount of industrial hemp is first removed from the hemp skin and sliced before being mixed into the coniferous wood chips. The pulping is done by the sulfate method, oxygen delignification, hydrogen peroxide bleaching and cleaning. The pulping requirements are: whiteness 27-31% ISO; Kappa number 36-42. The cleaned pulp is sent to the pulp storage tower and sent to the pulping system with clean water. The poplar raw material is prepared and the PRC-APMP pulping process is used to make poplar chemical mechanical pulp with a whiteness of 76% ISO and a beating degree of 54-58°SR.
[0065] Beating: Beat the prepared pulp in three mills in series. Beating concentration: 3.6-4%. Beating is mainly for decomposition and brooming. In principle, less cutting is required. NBKP and LBKP are beaten with 0.4-0.8kg / t of sodium carboxymethyl cellulose (CMC). The freeness of the pulp after beating is 275-325ml for coniferous pulp, 285-335ml for broadleaf pulp, and 200-230ml for poplar chemical mechanical pulp.
[0066] The three pulps are mixed in the ratio of 25%:20%:55%; then 12% filler-grade light calcium carbonate (grade 60) filler is added, and sent to the first-stage four-stage conical slag remover for purification and slag removal through a slurry pump, and then enter the degassing tank for degassing; then enter the pressure screen for screening (cationic PAM dosage 0.6kg / ton paper, cationic starch 10kg / ton paper, both added at the pressure screen inlet, modified diatomaceous earth 2.8kg / ton paper, added at the pressure screen outlet).
[0067] Then the mixed slurry is sent to the headbox to be screened, and the screen flow is adjusted to control the scanned paper weight at 45g / m 2 Around; after the wet paper leaves the screen section, it enters the pressing section for five-roller three-pressure zone composite pressing. After being pressed to a dryness ≥ 39%, it enters the pre-drying section; the surface temperature of the drying cylinder is controlled at 90-130°C to dry the paper until the dryness of the paper is ≥ 95%.
[0068] Next, the paper sheet enters the coating machine for surface treatment on the front and back sides: the components of the front coating formula are by weight: 20 parts of Brazilian clay, 10 parts of aluminum oxide, 20 parts of talcum powder, 70 parts of coating grade heavy calcium carbonate (grade 95), 15 parts of styrene-butadiene latex, 0.2 parts of tricarboxylic acid copolymer (molecular weight 5000-8000, viscosity 100-400mpas), other trace additives in appropriate amounts, coating solid content 65-67%, defoamer in appropriate amounts; front coating amount 8g / m 2 ; The components of the reverse coating formula are by weight: 20 parts of Brazilian porcelain clay, 10 parts of aluminum oxide, 20 parts of talc, 70 parts of coating grade heavy calcium carbonate (grade 95), 15 parts of styrene-butadiene latex, 0.2 parts of tricarboxylic acid copolymer, appropriate amount of other trace additives, coating solid content 65-67%, appropriate amount of defoamer; reverse coating amount 7g / m 2 The coating conditions are the same as in Example 1.
[0069] The coated paper sheets enter the post-drying process, and the dryness of the paper sheets out of the post-drying section is ≥93%; the paper sheets produced from the post-drying section enter the calendering area for calendering. The calender uses an 8-roller 7-nip pressure mode with a pressure of 210-245 kN / m; the calendering temperature of the 3 hot rollers is 185℃-245℃; after calendering, the paper is rolled up to obtain a basis weight of 56g / m 2 DM single paper with a whiteness of 82.0-84.0% ISO and a front gloss of 48% can fully meet the high-end usage requirements of customers. Other parameters of the paper machine are the same as those in Example 1.
[0070] Using the unified national standard testing method, the quality indicators of the DM single paper prepared in Example 1, Example 2 and Example 3 are summarized in the following table:
[0071] Table 2 DM single paper product indicators of Examples 1-3 of the present invention
[0072]
[0073]
[0074] As can be seen from the above table, the DM paper manufactured by the embodiment of the present invention has excellent physical indicators, among which the front gloss is between 42-48%, which is significantly better than the prior art (30-35%). The DM paper surface gloss, printing gloss, and surface strength of the embodiment of the present invention are significantly improved, the product quality is high, and the cost is low, which is of great significance to expanding the market for coating products and increasing product profit margins.
[0075] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0076] This article uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. The above is only a preferred implementation of the present invention. It should be pointed out that due to the limitations of textual expression and the objective existence of infinite specific structures, ordinary technicians in this technical field can make several improvements, modifications or changes without departing from the principles of the present invention, and can also combine the above technical features in an appropriate manner; these improvements, modifications, changes or combinations, or the direct application of the inventive concept and technical solution to other occasions without improvement, should be regarded as the protection scope of the present invention.
Claims
1. A method for manufacturing DM paper, characterized in that: The following steps are involved: Using bleached kraft softwood chemical pulp, bleached kraft hardwood chemical pulp and alkaline hydrogen peroxide poplar mechanical pulp as raw materials, the process is followed by beating, pulping and auxiliary material addition, wet paper sheet forming, pre-drying, coating and sizing, and post-drying to obtain DM single paper; the DM single paper has a basis weight of 48-64g / m 2 The DM paper has a front smoothness greater than 700s, a front roughness less than 1.7µm, and a front glossiness greater than or equal to 40%; The bleached kraft softwood chemical pulp is blended with industrial hemp, and the mass ratio of the bleached kraft softwood chemical pulp, the bleached kraft hardwood chemical pulp, and the alkaline hydrogen peroxide poplar mechanical pulp is 25-30%: 20-25%: 45-50%. After beating, the freeness of the bleached kraft softwood chemical pulp is 275-325 mL; the freeness of the bleached kraft hardwood chemical pulp is 285-335 mL; and the freeness of the alkaline hydrogen peroxide poplar mechanical pulp is 200-230 mL. The coating formulation used for the sizing includes, by weight, 10-20 parts of Brazilian clay, 5-10 parts of aluminum oxide, 15-20 parts of talc, 50-70 parts of coating-grade heavy calcium carbonate, 10-15 parts of styrene-butadiene latex, and 0.1-0.2 parts of a tricarboxylic acid copolymer; the tricarboxylic acid copolymer has a molecular weight of 5000-8000 and a room temperature viscosity of 100-400 mPa·s; the coating formulation also includes a defoamer; the solid content of the coating is 65-67%; the sizing is a double-sided coating process, and the total coating amount is 15-19 g / m 2 .
2. The method for manufacturing DM paper according to claim 1, characterized in that: The bleached kraft softwood chemical pulp and the bleached kraft hardwood chemical pulp are further pulped with 0.4-0.8 kg / t pulp of sodium carboxymethyl cellulose.
3. The method for manufacturing DM paper according to any one of claims 1 to 2, characterized in that: The components added into the auxiliary materials include fillers, cationic starch, polyacrylamide, bentonite and organic particles.
4. The method for manufacturing DM paper according to claim 3, characterized in that: Among the auxiliary materials, the weight ratio of filler is 8-10%; the weight ratio of cationic starch is 0.7-1.1%; and the weight ratio of bentonite is 0.15-0.35%.
5. The method for manufacturing DM paper according to any one of claims 1 to 2, characterized in that: During the double-sided coating process, the coating amount on the front side is greater than the coating amount on the back side.
6. The method for manufacturing DM paper according to any one of claims 1 to 2, characterized in that: The post-drying step also includes calendering, which adopts an 8-roller 7-nip pressure mode with a pressure of 200-250 kN / m.
7. The method for manufacturing DM paper according to claim 6, characterized in that: The moisture content of the paper sheet obtained by the post-drying is 6-9%.
8. The method for manufacturing DM paper according to claim 6, characterized in that: The calendering temperature is 180-250°C.
Citation Information
Patent Citations
Liquid packaging body paper board and preparation method thereof
CN103806326A
Production method of top-grade book white offset printing paper
CN105155332A
Method of manufacturing of bulky thickness micro-coated offset paper
CN107059462A
Thixotropic agents comprising ethylene terpolymer waxes
US20050131131A1