Zirconium dioxide / MXene composite filler modified epoxy resin anticorrosive coating and preparation method and application thereof
By surface modification of zirconium dioxide and combining with MXene to form composite fillers, the defects of epoxy resin coating and uneven dispersion of nanofillers during curing are solved, and the corrosion resistance and toughness are significantly improved, and the corrosion resistance and toughness are extended. The service life of the coating.
Patent Information
- Application Number
- CN202310863593.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-14
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-07-14
AI Technical Summary
The existing epoxy resin coatings are prone to defects during the curing process, causing corrosive media to enter the surface of the substrate, and the nanofillers are unevenly dispersed in the coating, limiting their corrosion resistance and toughness.
By surface modification of zirconium dioxide using silane coupling agent and combining with MXene to form a composite filler, add to carboxylated epoxy resin, improve the compatibility of nanofillers and epoxy resin, and form a self-assembled structure to delay delay The time when water enters the coating, enhancing corrosion resistance.
It significantly improves the corrosion resistance of the epoxy resin coating, enhances its toughness and adhesion, extends the service life of the coating, and improves the barrier performance of corrosive media.
Smart Images

Figure SMS_1 
Figure HDA0004338426230000011 
Figure HDA0004338426230000021
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of anti-corrosion coatings, and specifically relates to a zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating, and a preparation method and application thereof. Background Art
[0002] Metal corrosion is widespread in all fields, not only causing huge economic losses, but also having a serious impact on production safety. Most accidents that pose a major threat to safety, such as bridge ruptures and chemical pipeline leaks, are caused by metal corrosion. Among the many methods to prevent corrosion, coatings are the most widely used. Epoxy resins have excellent moisture resistance, resistance to corrosion by various solvents and chemicals, and good adhesion, and have always been a popular candidate for the development and application of corrosion-resistant coating systems. However, unmodified epoxy resins are relatively brittle, with low impact strength and toughness, which limits their widespread application in the field of coatings. Therefore, it is crucial to modify epoxy resins to improve their toughness and other functionalities. Nanomaterials play an inevitable role in the modification of epoxy resins, and epoxy resin systems with the addition of nanomaterials have significant improvements in toughening. There are many types of nanomaterials used for epoxy matrix toughening, including titanium dioxide, silicon dioxide, graphene, graphene oxide (GO), carbon nanotubes (CNT), etc. Among them, two-dimensional nanomaterials are now also very popular because their excellent performance stems from their high aspect ratio and specific surface area, surface chemistry and quantum size effect. The influence of surface modification of nanofillers and the interfacial interaction in polymer matrix is a field of great concern in current research, especially hybrid nanofillers, which play a significant role in changing the properties of polymers. Epoxy anticorrosive coatings have always been a hot topic of research because of the defects generated during the curing process, which make it easy for corrosive media to enter the contact substrate surface, and the nanofillers cannot be evenly dispersed in the coating. The present invention uses silane coupling agents to modify the surface of zirconium dioxide nanoparticles to solve the problem of easy agglomeration of nanoparticles. At the same time, the flake Ti 3 C 2 T X The addition of a self-contained structure, two-dimensional Ti 3 C 2 T X The nanosheets are dispersed in the gaps of the epoxy resin coating to form a maze effect, delaying the time it takes for water to enter the coating and contact the substrate, effectively extending the diffusion path of the corrosive medium in the coating and improving the anti-corrosion effect. Summary of the invention
[0003] In view of the problems mentioned in the background technology, the present invention improves the anti-corrosion performance of epoxy resin coatings, uses a silane coupling agent to modify nano zirconium dioxide and MXene, and adds them to a carboxylated epoxy resin matrix to prepare a coating with better anti-corrosion performance on the surface of the substrate. The present invention provides a method for preparing a carboxylated epoxy resin-nano zirconium dioxide / MXene anti-corrosion coating, which improves the problem of poor compatibility between nanofillers and epoxy resins, improves the anti-corrosion ability of the coating, and avoids the failure and precipitation of the coating during daily storage.
[0004] The purpose of the present invention is achieved through the following solutions:
[0005] The present invention provides a method for preparing a zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating, comprising the following steps:
[0006] (1) Zirconium dioxide / Ti 3 C 2 T X Preparation of composite filler: dissolve zirconium dioxide in an organic solvent, add a silane coupling agent to modify the zirconium dioxide, wash and dry the precipitate to obtain silane-modified zirconium dioxide, and then add the modified zirconium dioxide to Ti 3 C 2 T X After stirring the reaction in aqueous solution, the precipitated zirconium dioxide / Ti 3 C 2 T X The particles are washed and dried to obtain the zirconium dioxide / Ti 3 C 2 T X Composite fillers;
[0007] (2) Preparation of carboxylated epoxy resin: 1,3,5-benzenetricarboxylic acid, adipic acid and a solvent are mixed, then diglycidyl ether of bisphenol A and an initiator are added, reacted under heating conditions, and the precipitate is collected, washed and dried to obtain a modifier; the modifier is dispersed in the epoxy resin and stirred to obtain the carboxylated epoxy resin;
[0008] (3) Preparation of zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating: Add the composite filler obtained in step (1) to the carboxylated epoxy resin obtained in step (2) and stir evenly, then add an auxiliary agent and stir evenly to obtain component A; add an epoxy resin curing agent to component A and stir evenly to obtain the zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating.
[0009] Preferably, in step (2), the mass ratio of the modifier to the epoxy resin is 3 to 7:100;
[0010] In step (3), the mass ratio of zirconium dioxide / MXene composite filler to carboxylated epoxy resin is 1 to 4:100.
[0011] Preferably, in step (1), the organic solvent is toluene;
[0012] The silane coupling agent is 3-aminotriethoxysilane APTES;
[0013] The mass ratio of the silane coupling agent to zirconium dioxide is 2 to 3:1;
[0014] The modification treatment condition is reflux at 60±10°C for 24±6h;
[0015] The precipitate is washed multiple times with toluene and dichloromethane;
[0016] The stirring reaction conditions are: stirring reaction at a stirring speed of 500±100r / min for 1±0.5h;
[0017] The precipitated zirconium dioxide / Ti 3 C 2 T X The particles were washed several times with water.
[0018] Preferably, in step (2), the solvent is isobutyl alcohol; the initiator is triphenylphosphine;
[0019] The molar ratio of 1,3,5-benzenetricarboxylic acid to adipic acid is 2 to 4:1;
[0020] The mass ratio of the diglycidyl ether of bisphenol A to the initiator is 45 to 55:1;
[0021] The molar ratio of diglycidyl ether of bisphenol A: 1,3,5-benzenetricarboxylic acid: adipic acid is 1-3:2-4:1;
[0022] The precipitate is washed with ether, tetrahydrofuran and ethanol in sequence;
[0023] The drying condition is vacuum drying at 80±10°C for 6±2h;
[0024] The heating temperature is 110±20°C and the heating time is 24±6h;
[0025] The mass ratio of the modifier to the epoxy resin is 5 to 7:100;
[0026] The stirring condition is 60±10° C. for 1±0.5 h. 5. The preparation method according to claim 1, characterized in that in step (3), the auxiliary agent comprises an active diluent, a leveling agent, a defoaming agent, a rheological agent and an adhesion promoter.
[0027] Preferably, the zirconium dioxide in step (1) is prepared by the following steps: hydrolyzing a diluted zirconium dioxide precursor with aqueous ammonia, and after the hydrolysis is completed, continuously stirring at room temperature to polymerize the gel, and then drying and calcining the obtained gel to obtain the zirconium dioxide;
[0028] Ti in step (1) 3 C 2 T X It is prepared by the following steps: Ti 3 AlC 2 The powder is added to the HF aqueous solution and stirred for reaction. After the reaction is completed, the Ti 3 C 2 T X .
[0029] More preferably, in the method for preparing zirconium dioxide, the diluted zirconium dioxide precursor is obtained by diluting zirconium n-propoxide with n-propanol, and the volume ratio of n-propanol to zirconium n-propoxide is 2:1;
[0030] The condition for the completion of the hydrolysis is that the pH value of the hydrolysis system reaches 10 to 10.5;
[0031] The continuous stirring time is 1±0.5h;
[0032] The drying temperature is 110±20°C and the drying time is 12±3h;
[0033] The calcination temperature is 550±50° C. and the calcination time is 2±0.5 h.
[0034] More preferably, Ti 3 C 2 T X In the preparation method, the volume ratio of HF to water in the HF aqueous solution is 2:3;
[0035] The reaction temperature is 60±10°C and the reaction time is 2±0.5h;
[0036] The centrifuge used was 8000±1000rpm for 10±5min;
[0037] The washing is performed by washing with water for multiple times until the pH value of the supernatant reaches 6 to 7;
[0038] The drying is performed under vacuum at 80±10° C. for 24±6 h.
[0039] The present invention also provides a zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating prepared by the above preparation method.
[0040] The present invention also provides the application of the above-mentioned zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating in marine engineering and metal industry anti-corrosion.
[0041] The mechanism of the present invention is:
[0042] The present invention prepares Figure 1 The self-assembled ZrO2 / MXene hybrids shown were used to synthesize toughened epoxy nanocomposites using 3-aminopropyltriethoxysilane (APTES) to 2 The particles were surface modified, and the amino groups of APTES were further combined with Ti 3 C 2 T X The epoxy resin is modified by synthesized carboxyl-terminated hyperbranched polyester, wherein the terminal carboxyl group in the branched structure can be connected with the amino group in APTES, thereby strengthening the connection between the filler and the epoxy resin, increasing the impact resistance and other properties of the epoxy resin, and also improving the toughness of the epoxy resin.
[0043] The present invention has the following advantages and beneficial effects over the prior art:
[0044] (1) The present invention uses a synthetic carboxyl-terminated hyperbranched polyester to modify the epoxy resin, introduces carboxyl groups into the epoxy resin, and improves the tensile strength, adhesion and thermal properties of the epoxy resin. The modified epoxy resin contains abundant carboxyl groups and hydroxyl groups, which are generated by the ring-opening polymerization of the epoxy group. The terminal carboxyl group can be used as a curing agent and react with the epoxy group, and the hydroxyl group can accelerate the curing process of the epoxy system by initiating a polycondensation mechanism.
[0045] (2) There are still many spaces in the network structure formed by cross-linking and curing of epoxy resin. Adding fillers to it can fill the holes and enhance the physical properties of the resin material. The zirconium dioxide / MXene hybrid designed by the present invention, in which the 2D MXene nanofiller is conducive to the construction of an ordered structure in shape and size, thereby achieving better stress transfer and providing better barrier properties while maintaining multifunctionality. The addition of zirconium dioxide further improves the coating performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 for ZrO 2 and Ti 3 C 2 T XSchematic diagram of the self-assembled structure.
[0047] Figure 2 This is a synthetic route for carboxyl-terminated hyperbranched polyesters. DETAILED DESCRIPTION
[0048] The present invention is further described in detail below in conjunction with the examples, but the embodiments of the present invention are not limited thereto. If the specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0049] Unless otherwise specified, the reagents used in the examples can be purchased from the market.
[0050] Example 1
[0051] A method for preparing a zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating comprises the following steps:
[0052] (1) Zirconium dioxide / MXene composite filler:
[0053] (a) 5 ml of zirconium n-propoxide was added to 10 ml of n-propanol. Then, ammonia water was added dropwise under magnetic stirring to hydrolyze until the pH reached 10-10.5. After the hydrolysis was completed, stirring was continued at room temperature for 1 hour to polymerize the gel. Then, the obtained gel was placed in an oven at 110°C for 12 hours and finally calcined in a tubular furnace at 550°C for 2 hours to obtain zirconium dioxide powder.
[0054] (b) HF solution was used to etch and remove the MAX phase (Ti 3 AlC 2 ) to obtain a two-dimensional layered Ti 3 C 2 T X 8.3gTi 3 AlC 2 The powder was slowly added to a beaker containing 200 ml of HF (40%) aqueous solution and stirred in a 60°C constant temperature water bath for 2 h. After the reaction was completed, the mixture was centrifuged at 8000 rpm for 10 min and washed with deionized water several times until the pH of the supernatant was 6-7. The washed product was placed in a vacuum oven and dried to obtain a two-dimensional material.
[0055] (c) Weigh 1 g of zirconium dioxide powder, add it to 5 ml of toluene and ultrasonicate for 10 min. Then weigh 2.21 g of 3-aminotriethoxysilane and add it to the above solution, heat and reflux at 60°C for 24 h, wash the obtained precipitate with toluene and dichloromethane several times and dry it to obtain silane-modified zirconium dioxide powder. Then add the modified zirconium dioxide powder containing 1 g of Ti 3 C2 T X The precipitated zirconium dioxide / Ti 3 C 2 T X The particles were washed with water for several times and dried to obtain composite powder.
[0056] (2) Preparation of carboxyl-terminated hyperbranched polyester modifier:
[0057] 10.08 g of 1,3,5-benzenetricarboxylic acid, 2.33 g of adipic acid and 140 mL of isobutyl alcohol were placed in a round-bottom flask equipped with a magnetic stirrer and a condenser, and then 25 g of diglycidyl ether of bisphenol A and 0.5 g of triphenylphosphine were added to the mixture, and the mixture was stirred at 110° C. for 24 hours. Then, the precipitate was collected and washed with ether, tetrahydrofuran and ethanol in sequence, and the product was dried at 80° C. under vacuum to obtain a modifier.
[0058] (3) Preparation of carboxylated epoxy resin:
[0059] 2.5 g of the above modifier was weighed and dispersed in 50 g of epoxy resin, and mechanically stirred at 60° C. for 1 hour to make the mixture uniform to obtain carboxylated epoxy resin A.
[0060] (4) Preparation of modified epoxy resin anticorrosion coating:
[0061] Weigh 0.3g of zirconium dioxide / MXene composite filler and 10g of modified epoxy resin A into a beaker, stir at 600r / min for 2h to allow the filler to be evenly dispersed in the resin and connected to the resin, continue to add 3g of active diluent o-cresyl glycidyl ether, 1g of leveling agent polyacrylic acid, 0.25g of defoaming agent polydimethylsiloxane, 0.5g of rheological additive hydroxyethyl cellulose (HEC), and 0.5g of adhesion promoter phthalate into the beaker, stir for 30min to obtain component A; add 10g of polyamide curing agent to component A, stir for 30 minutes to obtain a composite filler modified epoxy anti-corrosion coating, apply it on the polished substrate and cure at room temperature to obtain an anti-corrosion coating.
[0062] Example 2
[0063] A method for preparing a zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating comprises the following steps:
[0064] (1) Zirconium dioxide / MXene composite filler: prepared in the same manner as in Example 1
[0065] (2) Preparation of carboxyl-terminated hyperbranched polyester modifier: the same preparation method as in Example 1
[0066] (3) Preparation of carboxylated epoxy resin:
[0067] 1.5 g of the above modifier was weighed and dispersed in 50 g of epoxy resin, and mechanically stirred at 60° C. for 1 hour to make the mixture uniform to obtain carboxylated epoxy resin B.
[0068] (4) Preparation of modified epoxy resin anticorrosion coating:
[0069] Weigh 0.3g of zirconium dioxide / MXene composite filler and 10g of modified epoxy resin B into a beaker, stir at 600r / min for 2h to allow the filler to be evenly dispersed in the resin and connected to the resin, continue to add 3g of active diluent o-cresyl glycidyl ether, 1g of leveling agent polyacrylic acid, 0.25g of defoaming agent polydimethylsiloxane, 0.5g of rheological additive hydroxyethyl cellulose (HEC), and 0.5g of adhesion promoter phthalate into the beaker, stir for 30min to obtain component A; add 10g of polyamide curing agent to component A, stir for 30 minutes to obtain a composite filler modified epoxy anti-corrosion coating, apply it on the polished substrate and cure at room temperature to obtain an anti-corrosion coating.
[0070] Example 3
[0071] A method for preparing a zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating comprises the following steps:
[0072] (1) Zirconium dioxide / MXene composite filler: prepared in the same manner as in Example 1
[0073] (2) Preparation of carboxyl-terminated hyperbranched polyester modifier: the same preparation method as in Example 1
[0074] (3) Preparation of carboxylated epoxy resin:
[0075] 3.5 g of the above modifier was weighed and dispersed in 50 g of epoxy resin, and mechanically stirred at 60° C. for 1 hour to make the mixture uniform to obtain carboxylated epoxy resin C.
[0076] (4) Preparation of modified epoxy resin anticorrosion coating:
[0077] Weigh 0.3g of zirconium dioxide / MXene composite filler and 10g of modified epoxy resin C into a beaker, stir at 600r / min for 2h to allow the filler to be evenly dispersed in the resin and connected to the resin, continue to add 3g of active diluent o-cresyl glycidyl ether, 1g of leveling agent polyacrylic acid, 0.25g of defoaming agent polydimethylsiloxane, 0.5g of rheological additive hydroxyethyl cellulose (HEC), and 0.5g of adhesion promoter phthalate into the beaker, stir for 30min to obtain component A; add 10g of polyamide curing agent to component A, stir for 30 minutes to obtain a composite filler modified epoxy anti-corrosion coating, apply it on the polished substrate and cure at room temperature to obtain an anti-corrosion coating.
[0078] Example 4
[0079] A method for preparing a zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating is the same as Example 1 except for the following steps: In the preparation of (4) the modified epoxy resin anti-corrosion coating, 0.1 g of zirconium dioxide / MXene composite filler and 10 g of modified epoxy resin are weighed into a beaker and stirred at 600 r / min for 2 h so that the filler can be evenly dispersed in the resin and connected to the resin.
[0080] Example 5
[0081] A method for preparing a zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating is the same as Example 1 except for the following steps: In the preparation of (4) the modified epoxy resin anti-corrosion coating, 0.2 g of zirconium dioxide / MXene composite filler and 10 g of modified epoxy resin are weighed into a beaker and stirred at 600 r / min for 2 h so that the filler can be evenly dispersed in the resin and connected to the resin.
[0082] Example 6
[0083] A method for preparing a zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating is the same as Example 1 except for the following steps: In the preparation of (4) the modified epoxy resin anti-corrosion coating, 0.4 g of zirconium dioxide / MXene composite filler and 10 g of modified epoxy resin are weighed into a beaker and stirred at 600 r / min for 2 h so that the filler can be evenly dispersed in the resin and connected to the resin.
[0084] Comparative Example 1
[0085] A method for preparing an unmodified epoxy resin anticorrosive coating comprises the following steps:
[0086] Weigh 10g of unmodified epoxy resin into a beaker, and continue to add 3g of active diluent o-cresyl glycidyl ether, 1g of leveling agent polyacrylic acid, 0.25g of defoaming agent polydimethylsiloxane, 0.5g of rheological additive hydroxyethyl cellulose (HEC), and 0.5g of adhesion promoter phthalate into the beaker, and stir for 30 minutes to obtain component A; add 10g of polyamide curing agent to component A, stir for 30 minutes to obtain unmodified epoxy anti-corrosion coating, apply it on the polished substrate and cure at room temperature to obtain an anti-corrosion coating.
[0087] Comparative Example 2
[0088] A method for preparing an MXene filler-modified epoxy resin anticorrosive coating comprises the following steps:
[0089] Weigh 0.3g of Mxene filler and 10g of carboxylated epoxy resin A into a beaker, and continue to add 3g of active diluent o-cresyl glycidyl ether, 1g of leveling agent polyacrylic acid, 0.25g of defoaming agent polydimethylsiloxane, 0.5g of rheological additive hydroxyethyl cellulose (HEC), and 0.5g of adhesion promoter phthalate into the beaker, and stir for 30 minutes to obtain component A; add 10g of polyamide curing agent to component A, stir for 30 minutes to obtain a modified epoxy anti-corrosion coating, apply it on the polished substrate and cure it at room temperature to obtain an anti-corrosion coating.
[0090] Comparative Example 3
[0091] A method for preparing a zirconium dioxide filler modified epoxy resin anti-corrosion coating comprises the following steps:
[0092] Weigh 0.3 g of zirconium dioxide filler and 10 g of carboxylated epoxy resin A into a beaker, and continue to add 3 g of active diluent o-cresyl glycidyl ether, 1 g of leveling agent polyacrylic acid, 0.25 g of defoaming agent polydimethylsiloxane, 0.5 g of rheological additive hydroxyethyl cellulose (HEC), and 0.5 g of adhesion promoter phthalate into the beaker, and stir for 30 minutes to obtain component A; add 10 g of polyamide curing agent to component A, stir for 30 minutes to obtain a modified epoxy anti-corrosion coating, apply it on the polished substrate and cure at room temperature to obtain an anti-corrosion coating.
[0093] Performance Testing
[0094] The performance of Examples 1 to 6 and Comparative Examples 1, 2, and 3 was tested according to the following test method. The test results are shown in Table 1.
[0095] (1) Electrochemical impedance performance test: The zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating prepared in Examples 1-6 and Comparative Examples 1, 2, and 3 was coated on a treated circular carbon steel electrode with a diameter of 1 cm and cured at room temperature for 72 h. The obtained electrode was immersed in a 3.5% NaCl solution and the electrochemical impedance was tested for 1 day, 10 days, and 30 days, respectively.
[0096] (2) Adhesion (pull-off method): Test standard GB / T 5219-2006.
[0097] (3) Hardness: Test standard GB / T 6739-2006.
[0098] (4) Impact resistance: Test standard GB / T 1732-2020.
[0099] (5) Flexibility: Test standard GB / T 1731-2020.
[0100] (6) Neutral salt spray resistance: Test standard GB / T 1771-2007.
[0101] (7) Alkali resistance (5% NaOH): test standard GB / T 9274-1988.
[0102] (8) Salt water resistance (5% NaCl): test standard GB / T 9274-1988.
[0103] (9) Water resistance (90℃~100℃): Test standard GB / T 1733-1993.
[0104] Epoxy resin coating test results: Table 1
[0105]
[0106] As can be seen from the table, carboxyl-modified epoxy resin can effectively improve the impact resistance and flexibility of the coating. The optimal doping ratio of zirconium dioxide / MXene as a filler in the coating can further extend the route for water to enter the coating and contact the substrate compared to zirconium dioxide or MXene single filler, which can improve the impedance value of the coating and improve its corrosion resistance. Compared with the common epoxy anti-corrosion coatings on the market, the coating prepared by the present invention has better physical properties and excellent corrosion resistance, and its adhesion is much higher than that of conventional coatings, and can be used for corrosion protection under more extreme conditions.
[0107] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a zirconium dioxide / MXene composite filler modified epoxy resin anticorrosive coating, characterized in that: The following steps are involved: (1) Zirconium dioxide / Ti3C2T X Preparation of composite filler: dissolve zirconium dioxide in an organic solvent, add a silane coupling agent to modify the zirconium dioxide, wash and dry the precipitate to obtain silane-modified zirconium dioxide, and then add the modified zirconium dioxide to Ti3C2T X After stirring the reaction in aqueous solution, the precipitated zirconium dioxide / Ti3C2T X The particles are washed and dried to obtain the zirconium dioxide / Ti3C2T X Composite fillers; (2) Preparation of carboxylated epoxy resin: 1,3,5-benzenetricarboxylic acid, adipic acid and a solvent are mixed, then diglycidyl ether of bisphenol A and an initiator are added, reacted under heating conditions, and the precipitate is collected, washed and dried to obtain a modifier; the modifier is dispersed in the epoxy resin and stirred to obtain the carboxylated epoxy resin; (3) Preparation of zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating: Add the composite filler obtained in step (1) to the carboxylated epoxy resin obtained in step (2) and stir evenly, then add an auxiliary agent and stir evenly to obtain component A; add an epoxy resin curing agent to component A and stir evenly to obtain the zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating.
2. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of the modifier to the epoxy resin is 3 to 7:100; In step (3), the mass ratio of zirconium dioxide / MXene composite filler to carboxylated epoxy resin is 1 to 4:
100.
3. The preparation method according to claim 1, characterized in that: In step (1), the organic solvent is toluene; The silane coupling agent is 3-aminotriethoxysilane APTES; The mass ratio of the silane coupling agent to zirconium dioxide is 2 to 3:1; The modification treatment condition is reflux at 60±10°C for 24±6h; The precipitate is washed multiple times with toluene and dichloromethane; The stirring reaction conditions are: stirring reaction at a stirring speed of 500±100r / min for 1±0.5h; The precipitated zirconium dioxide / Ti3C2T X The particles were washed several times with water.
4. The preparation method according to claim 1, characterized in that: In step (2), the solvent is isobutyl alcohol; the initiator is triphenylphosphine; The molar ratio of 1,3,5-benzenetricarboxylic acid to adipic acid is 2 to 4:1; The mass ratio of the diglycidyl ether of bisphenol A to the initiator is 45 to 55:1; The molar ratio of diglycidyl ether of bisphenol A: 1,3,5-benzenetricarboxylic acid: adipic acid is 1-3:2-4:1; The precipitate is washed with ether, tetrahydrofuran and ethanol in sequence; The drying condition is vacuum drying at 80±10°C for 6±2h; The heating temperature is 110±20°C and the heating time is 24±6h; The mass ratio of the modifier to the epoxy resin is 5 to 7:100; The stirring condition is stirring at 60±10° C. for 1±0.5 h.
5. The preparation method according to claim 1, characterized in that: In step (3), the auxiliary agents include active diluents, leveling agents, defoaming agents, rheological additives and adhesion promoters.
6. The preparation method according to claim 1, characterized in that: The zirconium dioxide in step (1) is prepared by the following steps: hydrolyzing a diluted zirconium dioxide precursor with aqueous ammonia, and after the hydrolysis is completed, continuously stirring at room temperature to polymerize the gel, and then drying and calcining the obtained gel to obtain the zirconium dioxide; Ti3C2T in step (1) X The Ti3AlC2 powder is added to the HF aqueous solution and stirred for reaction. After the reaction is completed, the powder is centrifuged, washed and dried to obtain the Ti3C2T X .
7. The preparation method according to claim 6, characterized in that: In the preparation method of zirconium dioxide, the diluted zirconium dioxide precursor is obtained by diluting zirconium n-propoxide with n-propanol, and the volume ratio of n-propanol to zirconium n-propoxide is 2:1; The condition for the completion of the hydrolysis is that the pH value of the hydrolysis system reaches 10 to 10.5; The continuous stirring time is 1±0.5h; The drying temperature is 110±20°C and the drying time is 12±3h; The calcination temperature is 550±50° C. and the calcination time is 2±0.5 h.
8. The preparation method according to claim 6, characterized in that: Ti3C2T X In the preparation method, the volume ratio of HF: water in the HF aqueous solution is 2:3; The reaction temperature is 60±10°C and the reaction time is 2±0.5h; The centrifuge used was 8000±1000rpm for 10±5min; The washing is performed by washing with water for multiple times until the pH value of the supernatant reaches 6 to 7; The drying is performed under vacuum at 80±10° C. for 24±6 h.
9. A zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating prepared by the preparation method according to any one of claims 1 to 8.
10. Application of the zirconium dioxide / MXene composite filler modified epoxy resin anti-corrosion coating according to claim 9 in marine engineering and metal industry anti-corrosion.
Citation Information
Patent Citations
Glass fiber powder / polypyrrole / Ti<3>C<2>T<x>MXene ternary composite filler, and preparation method and application thereof
CN110734659A
MXene and carbon nano tube synergistically modified polyurethane anticorrosive paint as well as preparation method and construction process thereof
CN114276743A