A method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase

By adding Mn elements to the magnesium alloy and adopting argon protection and spray casting process, the problem of insufficient precipitation phase density in the magnesium alloy is solved, and a high-density and uniform distribution of γ-precipitation phase is achieved, which improves the magnesium The performance of the alloy and reduce costs.

CN117107094BActive Publication Date: 2024-11-29GUANGDONG INST OF NEW MATERIALS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311022910.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-15
Publication Date
2024-11-29
Estimated Expiration
2043-08-15

AI Technical Summary

Technical Problem

The prior art is difficult to form a high-density γ″ substrate precipitation phase in magnesium alloys, and the processing time is long, limiting the performance and cost-effectiveness of the alloy.

Method used

By adding Mn elements to the Mg-Gd-Y-Zn alloy, using protective gas argon for smelting and spray casting, and then heating at 150-250°C for 50-200 hours to promote the precipitation phase of the γ-" substrate surface Form and distribution evenly.

Benefits of technology

The high-density, uniform γ″ substrate precipitation phase in Mg-Gd-Y-Zn-Mn alloy is realized, reducing costs and improving the mechanical properties and application value of magnesium alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117107094B_ABST
    Figure CN117107094B_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase, and belongs to the technical field of magnesium alloys. The method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase provided by the invention comprises: smelting and casting a metal raw material in a protective gas to obtain a master alloy; heating and melting the master alloy in the protective gas, and spray-casting the master alloy; then performing an artificial aging treatment, cooling, and obtaining the magnesium alloy containing the γ″ basal plane precipitation phase. The invention realizes the formation of a high-density, uniformly distributed γ″ basal plane precipitation phase in a Mg‑Gd‑Y‑Zn‑Mn alloy for the first time; the introduction of elements such as Mn and Y reduces the preparation cost, and promotes the strengthening of the γ″ basal plane precipitation phase, providing a new idea for the research, development, and preparation of high-performance, low-cost rare earth magnesium alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnesium alloys, and in particular to a method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase. Background Art

[0002] Magnesium alloys themselves have low interatomic bonding force and low strength, and precipitation phase transformation is an important way to strengthen magnesium alloys. In magnesium alloys, the size, morphology, and distribution of the precipitate phase have an important influence on the strengthening effect. The γ″ basal plane precipitate phase is a lamellar precipitate phase parallel to the basal plane of the magnesium matrix. Compared with the γ′ precipitate phase, it can more effectively hinder dislocation movement and is an important strengthening phase in magnesium alloys. At present, the formation of high-density γ″ basal plane precipitate phase stacking in magnesium alloys has only been reported in Mg-Gd(-Y)-Ag alloys; among them, the Ag element promotes the formation of high-density γ″ basal plane precipitate phase, but its cost is relatively high.

[0003] The Mn element can replace the more expensive Ag element and promote the formation of γ" basal plane precipitation phase in the magnesium alloy. CN115305373A discloses a method for forming a γ" basal plane precipitation phase in a magnesium alloy: adding the Mn element during the preparation of a Mg-Gd(-Y)-Zn magnesium alloy ingot, and then subjecting the magnesium alloy ingot to a solution treatment and an aging treatment in sequence, thereby obtaining a magnesium alloy containing a γ" basal plane precipitation phase. Although the above method can prepare a γ" basal plane precipitation phase at a relatively low cost, it does not achieve the formation of a high-density γ" basal plane precipitation phase in the magnesium alloy, and the processing time is relatively long, and there are still certain limitations in the synthesis of magnesium alloys and their application performance.

[0004] Since the Mn element plays an important role in the formation of the γ″ basal plane precipitation phase, in order to precipitate more γ″ phase in this alloy, it is necessary to increase the solubility of the Mn element in the magnesium matrix. However, due to the high melting point of Mn (~1244°C) and its low solubility in magnesium, it is difficult to make the Mn element solid-dissolve in the magnesium matrix in large quantities by conventional processes. This makes it difficult for magnesium alloys that replace Ag with Mn to achieve the formation of high-density γ″ basal plane precipitation phases.

[0005] Therefore, optimizing the solid solution of Mn in the magnesium matrix, improving the preparation process, and developing a method to form a high-density stacked γ″ precipitation phase magnesium alloy are of great significance for the research and development of high-performance and low-cost rare earth magnesium alloys. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a magnesium alloy containing a γ" basal plane precipitation phase, promote the formation of the γ" basal plane precipitation phase, and achieve high-density γ" basal plane precipitation in the Mg-Gd-Y-Zn-Mn alloy. The formed γ" basal plane precipitation phase is evenly and densely distributed in the magnesium alloy, and there is no particle precipitation on the surface of the magnesium alloy, and each component is fully dissolved, which provides a new idea for the research and development and preparation of high-performance, low-cost rare earth magnesium alloys.

[0007] To achieve the above object, the present invention adopts the following technical scheme. The present invention provides a method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase, comprising the following steps:

[0008] (1) melting and casting a metal raw material in a protective gas to obtain a master alloy; the metal raw material comprises the following metal elements: Mg, Gd, Y, Mn and Zn, and Mn accounts for 1-2.5% of the metal elements by mass percentage;

[0009] (2) Spray casting in protective gas;

[0010] (3) Heating at 150-250°C for 50-200h and then cooling to obtain a magnesium alloy containing a γ″ basal plane precipitation phase.

[0011] The metal raw materials are melted and cast to make the Mg, Mn, Gd, Y and Zn metal components in the raw materials fully mixed and uniform; the formed master alloy solid can maintain the uniform state after the first melting when remelting and recasting, which is convenient for subsequent processing.

[0012] The above raw material components form a Mg-Gd-Y-Zn-Mn alloy, in which Gd-Y-Zn-Mn can jointly constitute a γ" precipitation phase. When the Mn content is in the range of 1-2.5% by mass, the γ" basal plane precipitation can be promoted, and the γ" basal plane precipitation phase in the magnesium alloy is densely distributed. If the Mn content is too low, less γ" basal plane precipitation phase is formed; if the Mn content is too high, there are Mn particles that cannot be dissolved in solid and precipitate from the Mg matrix.

[0013] Through spray casting, the alloy solidifies quickly, which can refine the grains of the magnesium matrix and increase the solubility of Mn in the magnesium matrix; at the same time, the molten mother alloy is reshaped to form an oversaturated solidified body, which reduces the precipitation of Mn particles, makes it better dissolved in the alloy, promotes the formation of more γ″ basal plane precipitation phases, and shortens the required aging time.

[0014] Artificial aging treatment at 150-250℃ for 50-200h can eliminate the internal stress of magnesium alloy, stabilize the structure and size, and improve the mechanical properties: the magnesium alloy obtained by rapid solidification can precipitate a large amount of γ″ basal plane precipitation phase after aging treatment, which is evenly and densely distributed in the magnesium alloy. When the aging temperature is low and the aging time is short, the γ″ basal plane precipitation phase is less; when the aging time is too long, the distribution of the γ″ basal plane precipitation phase is reduced, and the γ′ basal plane precipitation phase increases.

[0015] The preparation method is simple to operate and has low raw material cost. It realizes high-density γ″ basal plane precipitation in the Mg-Gd-Y-Zn-Mn alloy, and its surface is uniform and no particles are precipitated. It has high application value in the research and development and preparation of high-performance and low-cost rare earth magnesium alloys.

[0016] Preferably, in step (1), the metal raw material includes the following components in mass percentage: 8-10% Gd, 4-5% Y, 1-1.5% Zn, 1-2.5% Mn, and the balance Mg. Within this component range, Gd, Y, Zn and Mn together constitute the γ″ basal plane precipitation phase of the magnesium alloy, with good solid solubility and no particle precipitation; and at this ratio, the content of the magnesium matrix component is high, retaining its good properties such as low density and good heat dissipation.

[0017] Preferably, in step (1), the smelting conditions are heating to 740°C, keeping warm and stirring for 10 minutes. After smelting, casting is performed at 730°C. Under the smelting conditions, the raw materials can be fully melted into liquid and uniformly mixed; stirring during the holding time makes the generated master alloy uniform in texture, which is convenient for remelting and recasting.

[0018] Preferably, in steps (1) and (2), the protective gas is argon. Argon is an inert gas and is insoluble in liquid metal at high temperatures, and can protect the metal components from oxidation.

[0019] Preferably, the process of spray casting in step (2) comprises: heating and melting the master alloy, vacuum spray casting, and cooling to form. In order to meet the requirements of spray casting, the master alloy needs to be heated and melted to a liquid state; vacuum spray casting is adopted, and the pressure difference generated by vacuuming is used, and the alloy liquid is sprayed into a collector or a mold under the dual effects of the pressure difference and gravity, and is rapidly cooled and solidified to form.

[0020] Further preferably, in step (2), the heating and melting temperature is 700-740° C. At this heating temperature, the master alloy melts rapidly and fully to form a flowing liquid, which meets the requirements of spray casting.

[0021] Further preferably, the vacuum condition in step (2) is 5×10 -3 -5×10 -4Pa vacuum degree. Under the above vacuum conditions, the molten alloy liquid can be quickly ejected from the nozzle under the combined action of pressure difference and gravity, enter the collector or mold, and quickly cool and solidify, reducing the precipitation of Mn particles and making it better dissolved in the magnesium matrix.

[0022] Preferably, in step (2), the cooling temperature is room temperature. The collector or mold temperature is controlled to be room temperature, at which point the ejected liquefied alloy rapidly cools and solidifies after contacting it, and the cooling rate can reach 10 4 K / s, during the rapid solidification process, the grains of the magnesium matrix are fully refined, and the solid solubility of Mn in the magnesium matrix is ​​improved.

[0023] Preferably, in step (3), the cooling method is water cooling at room temperature. After the aging treatment, the temperature is quickly reduced by water cooling to obtain a stable magnesium alloy product that is easy to store or reprocess.

[0024] Preferably, in step (3), heating is performed at 200-250° C. for 50-100 h. Under the artificial aging treatment conditions, the formed magnesium alloy can evenly precipitate a large amount of γ″ basal plane precipitation phase, reduce the formation of γ′ precipitation phase, and more effectively hinder the movement of dislocations, which is beneficial to the improvement of the strength of the magnesium alloy.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The preparation method of the present invention realizes uniform and high-density γ" basal plane precipitation phase in Mg-Gd-YZ-Mn alloy. Compared with adding expensive Ag to produce high-density γ" basal plane precipitation phase in magnesium alloy, the preparation method is optimized and the alloy cost is reduced. It has high application value in the research and development and preparation of high-performance and low-cost rare earth magnesium alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a conventional transmission electron microscope bright field image of a magnesium alloy containing γ″ basal precipitation phase;

[0028] Figure 2 Spherical aberration corrected HAADF-STEM image of magnesium alloy containing γ″ basal plane precipitation phase. DETAILED DESCRIPTION

[0029] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0030] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0031] Example 1

[0032] A method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase according to an embodiment of the present invention comprises the following specific steps:

[0033] (1) The following metal raw materials were prepared: pure Mg (99.9 wt.%), pure Zn (99.9 wt.%), Mg-30% Gd (wt.), Mg-25% Y (wt.), and Mg-10% Mn (wt.);

[0034] Weighing the metal raw materials so that, by mass percentage, they include 1.5% Mn, 8.75% Gd, 4.25% Y and 1.2% Zn, with the remainder being Mg;

[0035] Under argon protection, the metal raw material was heated to 740°C in an electromagnetic induction furnace, stirred and melted at 200 rpm, kept warm and stirred for 10 minutes, and cast at 730°C to obtain a master alloy;

[0036] (2) The master alloy is crushed into small pieces, the surface oxide layer is removed, and the pieces are placed in a quartz tube with a nozzle at the bottom, which is placed in the center of the heating coil of the induction melting furnace, while the nozzle is aimed at the copper mold cavity;

[0037] The inside of the copper mold was purged with argon gas and evacuated to a vacuum degree of 5×10 -4 Pa;

[0038] The furnace is filled with high-purity argon gas and induction heated to 740°C to fully melt the master alloy. Under the action of pressure difference and gravity, the liquid alloy is ejected from the nozzle and enters the copper mold cavity at room temperature, where it solidifies rapidly to obtain a formed magnesium alloy.

[0039] (3) The formed magnesium alloy is subjected to artificial aging treatment at a temperature of 200°C for a holding time of 50 h, and then water-cooled at room temperature to prepare a magnesium alloy containing a γ″ basal plane precipitation phase.

[0040] The prepared magnesium alloy was observed using a transmission electron microscope with the incident beam direction of <11-20> Mg Bright field photographs of Figure 1 ; Spherical aberration correction-high angle annular dark field-scanning transmission electron microscopy (HAADF-STEM) was used to characterize at the atomic scale. The results are as follows Figure 2 .

[0041] from Figure 1 From the TEM image at a 20nm scale, it can be observed that hundreds of precipitation phase layers parallel to the basal plane are formed in the magnesium alloy, and their distribution is dense and uniform. Further observation of its atomic scale characterization shows that its atomic arrangement conforms to the morphological characteristics of the γ” precipitation phase, confirming that the high-density precipitation phase produced is the γ” basal plane precipitation phase ( Figure 1 The circled part is a γ” precipitated phase).

[0042] Example 2

[0043] The difference between Example 2 and Example 1 is that the metal raw materials, in terms of mass percentage, include 1% Mn, 10% Gd, 4% Y and 1.5% Zn, and the rest is Mg; the artificial aging temperature is 250° C., the holding time is 100 h, and the remaining steps are the same as in Example 1.

[0044] A large amount of γ″ precipitated phase parallel to the basal plane is formed in the prepared magnesium alloy, and its distribution is dense and uniform.

[0045] Example 3

[0046] The difference between Example 3 and Example 1 is that the metal raw materials, in terms of mass percentage, include 2.5% Mn, 8% Gd, 5% Y and 1% Zn, and the rest is Mg; the heating and melting temperature of the master alloy is 700°C, and the vacuum degree used in the spray casting is 5×10 -3 Pa; the artificial aging temperature is 220°C, the holding time is 75h, and the remaining steps are the same as in Example 1.

[0047] A large amount of γ″ precipitated phase parallel to the basal plane is formed in the prepared magnesium alloy, and its distribution is dense and uniform.

[0048] Example 4

[0049] The difference between Example 4 and Example 1 is that the heating melting temperature of the master alloy is 730° C.; the artificial aging temperature is 150° C., and the holding time is 200 h. The remaining steps are the same as those in Example 1.

[0050] A large number of γ″ precipitates parallel to the basal plane were formed in the prepared magnesium alloy, and their distribution was dense and uniform; at the same time, the formation of a small amount of γ′ precipitates was observed.

[0051] Example 5

[0052] The difference between Example 5 and Example 1 is that during the spray casting, the vacuum degree is 10 -4 Pa, the artificial aging temperature is 200° C., the holding time is 200 h, and the remaining steps are the same as those in Example 1.

[0053] A large number of γ″ precipitates parallel to the basal plane were formed in the prepared magnesium alloy, and their distribution was dense and uniform; at the same time, the formation of a small amount of γ′ precipitates was observed.

[0054] Comparative Example 1

[0055] The difference between Comparative Example 1 and Example 1 is that the metal raw materials, in terms of mass percentage, include 3.5% Mn, 7% Gd, 5.5% Y and 0.5% Zn, and the rest is Mg; the remaining steps are the same as those in Example 1.

[0056] A large amount of Mn particles precipitate on the surface of the prepared magnesium alloy and cannot be completely dissolved.

[0057] Comparative Example 2

[0058] The difference between Comparative Example 2 and Example 4 is that the prepared master alloy is solution-solutionized at 500° C. for 10 hours without spray casting, and the remaining steps are the same as those in Example 1.

[0059] Only four γ″ precipitation phases were observed in the prepared magnesium alloy at a scale of 100 nm.

[0060] Comparative Example 3

[0061] The difference between Comparative Example 3 and Example 1 is that the artificial aging temperature is 200° C., the holding time is 30 h, and the remaining steps are the same as those in Example 1.

[0062] In the prepared magnesium alloy, only dozens of γ″ precipitation phases were observed at a scale of 100 nm.

[0063] Comparative Example 4

[0064] The difference between Comparative Example 3 and Example 1 is that the artificial aging temperature is 200° C. and the holding time is 250 h. The remaining steps are the same as those of Example 1.

[0065] In the prepared magnesium alloy, only dozens of γ″ precipitation phases were observed to form at the 100nm scale, but a large number of γ′ precipitation phases were formed and distributed near the γ″ basal plane precipitation phase.

[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase, characterized in that: It consists of the following steps: (1) melting and casting a metal raw material in a protective gas to obtain a master alloy; the metal raw material comprises the following components by mass percentage: 8-10% Gd, 4-5% Y, 1-1.5% Zn, 1-2.5% Mn, and the balance Mg; (2) Spray casting in protective gas; (3) heating at 200-250° C. for 50-100 h, and then cooling to obtain the magnesium alloy containing the γ″ basal plane precipitation phase.

2. The method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase according to claim 1, characterized in that: In the step (1), the smelting conditions are: heating to 740° C., keeping warm and stirring for 10 minutes.

3. The method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase according to claim 1, characterized in that: In the steps (1) and (2), the protective gas is argon.

4. The method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase according to claim 1, characterized in that: The process of the spray casting in step (2) comprises: heating and melting the master alloy, vacuum spray casting, and cooling to form the master alloy.

5. The method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase according to claim 4, characterized in that: In the step (2), the heating and melting temperature is 700-740°C.

6. The method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase according to claim 4, characterized in that: In step (2), the vacuum condition is 5×10 -3 -5×10 -4 Pa vacuum degree.

7. The method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase according to claim 4, characterized in that: In the step (2), the cooling temperature is room temperature.

8. The method for preparing a magnesium alloy containing a γ″ basal plane precipitation phase according to claim 1, characterized in that: In the step (3), the cooling method is water cooling at room temperature.

Citation Information

Patent Citations

  • Super-strength high-toughness magnesium alloy material and preparation method thereof

    CN103805821A

  • Method for forming magnesium alloy basal plane precipitated phase

    CN115305373A