Secondary battery and power-using device

Through the combination of specific electrolyte and negative electrode diaphragm resistivity parameters, the problem of reduced capacity and insufficient thermal stability of lithium-ion secondary batteries during large-scale charging is solved, and the dynamics and safety performance is improved, which is suitable for fast charging scenarios .

CN117613356BActive Publication Date: 2024-11-05SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311598064.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-27
Publication Date
2024-11-05
Estimated Expiration
2043-11-27

AI Technical Summary

Technical Problem

The material polarization effect of lithium-ion secondary batteries leads to a decrease in actual capacity during large-scale charging. During the charging process, the overpotential of lithium-ion graphite causes the electrode potential to drop to 0V, affecting service life and increasing the risk of internal short circuit, and insufficient thermal stability , easily lead to thermal runaway.

Method used

The electrolyte with specific properties and the resistivity parameters of the negative electrode diaphragm are used to improve the wetting ability of the electrolyte in the negative electrode and the electron conduction ability, reduce interface side reactions, and improve ion conduction ability. It is suitable for fast charging scenarios.

Benefits of technology

It improves the dynamic performance and safety performance of lithium-ion secondary batteries, reduces high-temperature gas production and internal short circuit risk, and is suitable for fast charging applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0004574884230000021
    Figure BDA0004574884230000021
  • Figure BDA0004574884230000041
    Figure BDA0004574884230000041
Patent Text Reader

Abstract

The present invention discloses a secondary battery and an electrical device, belonging to the field of energy storage. In the secondary battery of the present invention, high-viscosity and low-viscosity solvents are matched, and specific types of electrolyte additives are compounded at the same time, and a parameter relationship is jointly constructed with the resistivity of the negative electrode membrane, so that the overall electrolyte injection amount is increased without affecting the negative electrode electronic conduction, thereby improving the electrolyte infiltration effect; on the other hand, the unique electrolyte component selection can make the electrolyte have a low degree of interface side reaction when the secondary battery is working, the probability of gas production at room temperature or high temperature is small, and the ion conductivity is strong; the secondary battery has excellent kinetic performance, low risk of high-temperature gas production and DCR growth, and has ideal fast charging application performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a secondary battery and an electrical device. Background Art

[0002] Secondary batteries, especially lithium-ion secondary batteries, have always been one of the technical bottlenecks for power batteries due to their insufficient rate performance. Especially when charging at high rates, the polarization effect of various materials greatly reduces the actual capacity of the battery. On the other hand, the overpotential of lithium-ion graphite during charging is large, causing the electrode potential to drop below 0V. Lithium metal will be deposited at the negative electrode, affecting the battery's service life and increasing the risk of internal short circuits. In addition, the thermal stability of existing lithium-ion secondary batteries needs to be improved, and thermal runaway risks are prone to occur in some fast-charging applications.

[0003] In order to improve the overall performance of lithium-ion secondary batteries, researchers will modify the electrolyte or the negative electrode so that the electrolyte or the negative electrode can effectively cope with fast charging scenarios. However, these modified products are developed under laboratory conditions and have not undergone integration and actual simulation. When applied to actual full batteries, these products cannot perform at the same performance as under laboratory conditions. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a secondary battery and an electrical device. The secondary battery of the present invention is based on the selection of an electrolyte with specific properties, and at the same time, cooperates with the parameter relationship of the membrane resistivity of the negative electrode plate in the actual scenario, which can effectively improve the wettability of the electrolyte in the negative electrode, while ensuring that the electronic conductivity of the negative electrode itself will not decrease; the electrolyte has a low degree of interfacial side reactions when the secondary battery is working, a small probability of gas production at room temperature or high temperature, and a strong ion conductivity; the secondary battery has excellent kinetic performance and good safety performance, and is very suitable for fast charging scenarios.

[0005] To achieve the above object, in a first aspect of the present invention, the present invention provides a secondary battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the electrolyte comprises a solvent and an additive; the additive comprises a first additive, a second additive and a third additive; the solvent comprises a low-viscosity organic solvent and a high-viscosity organic solvent, wherein the viscosity of the low-viscosity organic solvent is ≤0.7 mPa.s, and the viscosity of the high-viscosity organic solvent is >0.7 mPa.s;

[0006] The secondary battery meets the following requirements:

[0007]

[0008] Wherein, the IC g / Ah is the injection coefficient of the electrolyte;

[0009] The EΩ / cm is the film resistivity of the negative electrode, d=6.70;

[0010] R is the mass ratio of the low-viscosity organic solvent to the total amount of solvent in the electrolyte;

[0011] The α is the mass percentage of the first additive in the electrolyte;

[0012] The β is the mass percentage of the second additive in the electrolyte;

[0013] The γ is the mass percentage of the third additive in the electrolyte;

[0014] The first additive includes a carbonate compound; the second additive includes a sulfur-based compound; and the third additive includes a phosphorus-based compound and / or a boron-based compound.

[0015] As an embodiment of the present invention, the secondary battery satisfies at least one of the following conditions:

[0016] (1) 2.30≤IC≤2.80;

[0017] (2) 0.210 ≤ E ≤ 0.253;

[0018] (3) 0.40≤R≤0.80;

[0019] (4) 0.1% ≤ α ≤ 1.0%;

[0020] (5) 0.1% ≤ β ≤ 3.0%;

[0021] (6)0.1%≤γ≤2%.

[0022] As an embodiment of the present invention, the low viscosity organic solvent includes at least one of dimethyl carbonate, ethyl methyl carbonate, methyl acetate, methyl propionate, methyl butyrate, methyl acetate, ethyl acetate, propyl acetate, ethyl butyrate and propyl propionate.

[0023] As an embodiment of the present invention, the secondary battery satisfies at least one of the following conditions:

[0024] (1) The carbonate compound includes at least one of vinylene carbonate and fluoroethylene carbonate;

[0025] (2) The sulfide compound includes at least one of vinyl sulfate, 1,3-propane sultone, propenyl-1,3-sultone, ethylene sulfite, methylene methane disulfonate, and 1,4-butane sultone;

[0026] (3) The phosphorus-based compound includes at least one of tris(trimethylsilyl)phosphate and lithium difluorophosphate;

[0027] (4) The boron-based compound includes lithium difluorooxalatoborate.

[0028] As an embodiment of the present invention, the high-viscosity organic solvent includes at least one of ethylene carbonate, propylene carbonate, butylene carbonate, diethyl carbonate, methylpropyl carbonate, diphenyl carbonate, and γ-butyrolactone.

[0029] As an embodiment of the present invention, the high-viscosity organic solvent comprises at least one of ethylene carbonate, propylene carbonate, and diethyl carbonate, and the low-viscosity organic solvent comprises ethyl methyl carbonate and / or ethyl acetate.

[0030] As an embodiment of the present invention, the α:β=0.25-0.5.

[0031] As an embodiment of the present invention, the negative electrode sheet contains a negative electrode active material, and the negative electrode active material.

[0032] In a second aspect of the present invention, the present invention provides an electric device, comprising the secondary battery, wherein the secondary battery serves as a power supply for the electric device.

[0033] The beneficial effects of the present invention are:

[0034] The present invention provides a secondary battery and an electrical device. In the secondary battery of the present invention, high-viscosity and low-viscosity solvents are matched, and specific types of electrolyte additives are compounded at the same time, and in conjunction with the negative electrode membrane resistance, the overall electrolyte injection amount is increased without affecting the negative electrode electronic conduction, thereby improving the electrolyte infiltration effect; on the other hand, the unique electrolyte component selection can make the electrolyte have a low degree of interface side reactions when the secondary battery is working, a small amount of gas production at high temperature, and a strong ion conductivity; the secondary battery has excellent kinetic performance, low high-temperature gas production and DCR growth risks, and has ideal fast charging application performance. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0037] In the present invention, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0038] In the present invention, there is no particular limitation on the specific dispersion and stirring treatment methods.

[0039] The reagents or instruments used in the present invention without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.

[0040] The present invention is further described below with specific embodiments:

[0041] The embodiment of the present invention provides a secondary battery, comprising a positive electrode plate, a negative electrode plate, a separator and an electrolyte, wherein the electrolyte comprises a solvent and an additive; the additive comprises a first additive, a second additive and a third additive; the solvent comprises a low-viscosity organic solvent and a high-viscosity organic solvent, wherein the viscosity of the low-viscosity organic solvent is ≤0.7 mPa.s, and the viscosity of the high-viscosity organic solvent is >0.7 mPa.s;

[0042] The secondary battery meets the following requirements:

[0043]

[0044] Wherein, the IC g / Ah is the injection coefficient of the electrolyte;

[0045] The EΩ / cm is the film resistivity of the negative electrode, d=6.70;

[0046] R is the mass ratio of the low-viscosity organic solvent to the total amount of solvent in the electrolyte;

[0047] The α is the mass percentage of the first additive in the electrolyte;

[0048] The β is the mass percentage of the second additive in the electrolyte;

[0049] The γ is the mass percentage of the third additive in the electrolyte;

[0050] The first additive includes a carbonate compound; the second additive includes a sulfur-based compound; and the third additive includes a phosphorus-based compound and / or a boron-based compound.

[0051] The matching of lithium-ion secondary battery system is an important factor affecting lithium-ion secondary batteries, such as the matching effect between electrolyte and negative electrode, which affects the balance between electrochemical performance and safety performance of lithium-ion batteries. In the process of electrolyte injection and infiltration of negative electrode plates, there is a correlation between the particle gap of active material in the negative electrode plate and the infiltration effect of electrolyte. When the gap is within the appropriate range, the infiltration effect of electrolyte is better, and the lithium ion conductivity of electrolyte in the negative electrode is better; at the same time, it can ensure the electronic conductivity between particles. Therefore, coordinating the relationship between the two can effectively improve the electrochemical performance of the product. In addition, when the secondary battery is working, the electrolyte will lose and interface side reactions will occur, so it is necessary to fully consider whether it is sufficient in the battery. However, if the composition of the electrolyte is not properly selected, as the amount of electrolyte added increases, the interface impedance and the consumption of active lithium will increase, which is not conducive to the battery kinetic performance and cycle life. On the other hand, after the negative electrode sheet is rolled, more planes are parallel to the surface of the sheet, and the degree of contact between the active material particles and the degree of contact between the active material and the binder also change. At this time, the membrane resistivity of the negative electrode sheet changes compared to the penetration efficiency in the loose state when the current applied to the sheet is tested, and the membrane resistivity of the negative electrode sheet has a certain relationship with the permeation of the electrolyte and ion conduction, but the inventors found that the relationship between the membrane resistivity of the negative electrode sheet and the physical properties such as the compaction density is not the same (with the increase of the compaction density, the membrane resistivity of the negative electrode sheet does not change linearly). Therefore, the secondary battery of the present invention is based on the selection of electrolyte with specific properties, and at the same time cooperates with the parameter relationship between the membrane resistivity of the negative electrode, which can effectively improve the wettability of the electrolyte in the negative electrode, while ensuring that the electronic conductivity of the negative electrode itself will not decrease, and can also reduce the degree of interfacial side reactions of the electrolyte when the secondary battery is working, so that the battery has a small gas production at high temperature and a strong ion conductivity, so that the secondary battery has excellent kinetic performance and good safety performance, which is very suitable for fast charging scenarios.

[0052] In some embodiments, 2.30≤IC≤2.80; for example, the injection coefficient IC g / Ah of the electrolyte is in the range of one or any two of 2.30g / Ah, 2.35g / Ah, 2.40g / Ah, 2.45g / Ah, 2.50g / Ah, 2.55g / Ah, 2.60g / Ah, 2.65g / Ah, 2.70g / Ah, 2.75g / Ah, and 2.80g / Ah.

[0053] The filling coefficient of the electrolyte has a certain relationship with the performance of the secondary battery. When the filling coefficient is within the above range, the lithium ions in the charging and discharging process can be effectively conducted, ensuring the actual capacity of the secondary battery, and improving the service life of the secondary battery. It can also ensure that the secondary battery has a high energy density, thus helping to improve the comprehensive performance of the secondary battery.

[0054] Specifically, the IC test method is: weigh the total mass of the battery to get m1. Then drain the electrolyte in the battery, re-add dimethyl carbonate, fully infiltrate the inside of the battery, wash out the residual lithium salt, repeat three times, and then open the battery to 80℃ for 24h to ensure that the residual dimethyl carbonate solvent is completely removed, weigh the mass of the battery after baking, and get the dry battery mass m2. The original mass of the electrolyte in the battery is m=m1-m2. Let the battery design capacity be C, then the electrolyte injection coefficient IC=C / m.

[0055] In some embodiments, 0.210≤E≤0.253; the film resistivity EΩ / cm of the negative electrode plate is in the range of one or any two of 0.210Ω / cm, 0.215Ω / cm, 0.220Ω / cm, 0.225Ω / cm, 0.230Ω / cm, 0.240Ω / cm, 0.250Ω / cm, and 0.253Ω / cm.

[0056] As mentioned above, the lithium ion deintercalation efficiency in the negative electrode and the wettability of the electrolyte affect the membrane resistivity of the negative electrode plate. When the membrane resistivity of the negative electrode plate is set within the above range, it can effectively ensure that the secondary battery has a higher energy density and avoid ion transmission failure of the negative electrode plate.

[0057] The film resistivity of the negative electrode is directly tested by the four-probe method, specifically using the ST2258C multi-function digital four-probe tester, and the average value is obtained by three parallel measurements.

[0058] In some embodiments, 0.40≤R≤0.80; for example, the mass ratio R of the low viscosity organic solvent to the total amount of solvent in the electrolyte is in the range of one or any two of 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80.

[0059] R is the proportion of low-viscosity organic solvents in the electrolyte within the above range, which can ensure that the viscosity of the overall electrolyte is within a reasonable range, so that the electrolyte has better wettability on the electrode, is beneficial to the conduction of lithium ions, and reduces high-temperature gas production.

[0060] Specifically, the test method of R, α, β, and γ is: the content of each component in the electrolyte can be monitored by combining the electrolyte quantification, organic matter qualitative and ion component analysis methods. The reference standard for electrolyte quantification is GB / T9722-2006 "General Rules for Gas Chromatography of Chemical Reagents", and the specific test conditions are: detector FID, detector temperature 300°C, injection port temperature 250°C, split ratio 100:1, injection volume 0.2μL, chromatographic column: KB-200, 60m x0.32mm x 0.50μm. The reference standard for organic matter qualitative analysis is GB / T 9722-2006 "General Rules for Mass Spectrometry Analysis Methods", MS ion source temperature 230°C, injection port temperature 240°C, split ratio 150:1, injection volume 0.2μL, chromatographic column: HP-5MS, 30m x 0.32mm x 0.25μm. The reference standards for the ion component analysis method are GB / T19282-2014 "Analysis Method for Lithium Hexafluorophosphate Products" and GB / T 34672-2017 "General Rules for Ion Chromatography Determination". Electrolyte sample pretreatment: take 1g and dilute 100 times, eluent concentration: 4.1mmol / L Na2CO3&2.7mmol / LNaHCO3&20% acetonitrile&0.05mol / L methanesulfonic acid, test time: 65min. R can be obtained by adding the mass ratio of each low-viscosity solvent to the total solvent of the electrolyte. α, β, and γ can also be measured by the above method.

[0061] In some embodiments, 0.1%≤α≤1.0%; for example, α may be a range of one or any two of 0.1%, 0.2%, 0.3%, 0.5%, 0.8%, 1%. More preferably, 0.2%≤α≤0.5%.

[0062] In some embodiments, 0.1%≤β≤3.0%; for example, β may be a range of 0.1%, 0.2%, 0.3%, 0.5%, 0.8%, 1%, 2%, 3%, or any two of them. More preferably, 1%≤β≤1.5%.

[0063] In some embodiments, 0.1%≤γ≤2%; for example, γ may be a range of one or any two of 0.1%, 0.2%, 0.3%, 0.5%, 0.8%, 1%, 2%, 3%.

[0064] More preferably, 1%≤γ≤1.5%.

[0065] The α is the mass percentage of the first additive in the electrolyte, β is the mass percentage of the second additive in the electrolyte, and γ is the mass percentage of the third additive in the electrolyte. The three are used together and the content range is controlled, which can effectively improve the cycle performance of the secondary battery, reduce the risk of high-temperature gas production and DCR growth, and reduce the side reactions caused by the use of the additives alone. The three additives work together and check and balance each other. When within the range, the secondary battery can not only ensure cycle stability, but also have a low probability of high-temperature gas production and excellent kinetic performance, which is very suitable for fast charging conditions.

[0066] In some embodiments, the compaction density PD of the negative electrode sheet satisfies: 1.35 g / cm 3 ≤PD g / cm 3 ≤1.78g / cm 3 ; For example, it can be 1.35g / cm 3 , 1.40g / cm 3 , 1.45g / cm 3 , 1.50g / cm 3 , 1.55g / cm 3 , 1.60g / cm 3 , 1.65g / cm 3 , 1.70g / cm 3 , 1.78g / cm 3 The compaction density of the negative electrode sheet is related to the deintercalation efficiency of lithium ions in the negative electrode and the wettability of the electrolyte. When the compaction density of the negative electrode sheet is set in the above range, it can effectively reduce the risk of internal short circuit caused by the shedding of particles on the negative electrode sheet, and ensure that the secondary battery has a higher energy density. In some embodiments, the low-viscosity organic solvent includes at least one of dimethyl carbonate, ethyl methyl carbonate, methyl acetate, methyl propionate, methyl butyrate, methyl acetate, ethyl acetate, propyl acetate, ethyl butyrate and propyl propionate.

[0067] In some embodiments, the high viscosity organic solvent includes at least one of ethylene carbonate, propylene carbonate, butylene carbonate, diethyl carbonate, methylpropyl carbonate, diphenyl carbonate, and γ-butyrolactone.

[0068] In some embodiments, the carbonate compound includes at least one of vinylene carbonate, vinyl ethylene carbonate, and fluoroethylene carbonate.

[0069] In some embodiments, the sulfur-based compound includes at least one of vinyl sulfate, 1,3-propane sultone, propenyl-1,3-sultone, ethylene sulfite, methylene methanedisulfonate, and 1,4-butane sultone.

[0070] In some embodiments, the phosphorus-based compound includes at least one of tris(trimethylsilyl)phosphate, lithium difluorophosphate

[0071] In some embodiments, the boron-based compound includes lithium difluorooxalatoborate.

[0072] In the electrolyte, the combination of the three additives can not only effectively suppress the risk of high-temperature gas production caused by low-viscosity solvents, but also avoid the deterioration of the DCR performance of the secondary battery. In particular, the ratio under the parameter relationship described in the present invention can make the comprehensive electrochemical performance of the secondary battery better.

[0073] In some embodiments, the high-viscosity organic solvent comprises at least one of ethylene carbonate, propylene carbonate, and diethyl carbonate, and the low-viscosity organic solvent comprises ethyl methyl carbonate and / or ethyl acetate.

[0074] In some embodiments, the electrolyte includes an electrolyte salt, and the electrolyte salt includes at least one of lithium hexafluorophosphate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethylsulfonyl imide, lithium tetrafluoroborate, lithium perchlorate, lithium tetrafluorophosphate, lithium bisoxalatodifluorophosphate, and lithium bisoxalatoborate.

[0075] More preferably, the electrolyte salt is lithium hexafluorophosphate.

[0076] Lithium hexafluorophosphate has an ideal ion migration number and dissociation constant in the electrolyte system of the present invention, and also has better environmental resistance and electrode adaptability.

[0077] More preferably, the mass content of the electrolyte salt in the electrolyte is 10-20 wt %.

[0078] In some embodiments, the α:β=0.25-0.5.

[0079] When the ratio of the first additive to the second additive is within the above range, the cycle life of the secondary battery can be further improved, and the safety performance of the secondary battery is better and the high-temperature gas generation level is lower.

[0080] More preferably, the α:γ=0.12-0.5; the β:γ=0.6-1.5. When this condition is met, the comprehensive electrochemical performance of the secondary battery can be further optimized.

[0081] In some embodiments, the negative electrode sheet contains a negative electrode active material, and the negative electrode active material includes a graphite material.

[0082] Further preferably, the particle size Dv of the graphite material is 50 The particle size Dv of the graphite material90 The ratio is 0.5 to 0.75. Dv 50 is the particle size corresponding to when the volume cumulative distribution percentage of the graphite material reaches 50%, Dv 90 is the particle size corresponding to when the volume cumulative distribution percentage of the graphite material reaches 90%.

[0083] Further preferably, the particle size Dv of the graphite material 50 ≤ 15 μm, and the particle size Dv of the graphite material 90 ≤ 25 μm.

[0084] The particle size Dv of the graphite material 50 and the Dv of the graphite material 90 can be obtained by testing with a laser particle size analyzer.

[0085] The inventors found through experiments that when in the electrolyte system of the present invention, graphite materials with different particle size distributions also have different degrees of balance in their wettability to the electrolyte and their own conductivity. When the particle size distribution is within a reasonable range, it can avoid the shedding of some small particles during charge and discharge, which affects the conductivity and cycle performance of the secondary battery. Moreover, when the particle size distribution is within a reasonable range, it can improve the impregnation performance of the negative electrode sheet to the electrolyte. When the graphite material within the above range is used as the negative electrode active material, the secondary battery can exhibit better performance in use.

[0086] In some embodiments, the positive electrode sheet includes a positive electrode active material layer, and the positive electrode active material layer contains a compound with the chemical formula Li a Ni x Co y M z O2, where M is selected from at least one of Mn, Al, Zr, Ti, V, Mg, Fe, B, and Mo, 0.95 ≤ a ≤ 1.2, 0.33 ≤ x < 1, 0 < y ≤ 0.33, 0 < z ≤ 0.33, and x + y + z = 1.

[0087] The present invention also provides an electrical device that uses the above secondary battery as a power supply. Since the above secondary battery has better cycle performance and lower gas generation performance, the electrical device has a longer endurance and better safety performance.

[0088] The following further elaborates the present invention with specific examples, and these examples should not be construed as limiting the scope claimed by the present invention:

[0089] Example 1

[0090] A secondary battery, and the preparation method includes the following steps:

[0091] (1) The positive electrode active material Li(Ni 0.8 Mn 0.1 Co 0.1 )O2(NMC811), conductive agent acetylene black (SuperP) and binder polyvinylidene fluoride (PVDF) were mixed uniformly in a mass ratio of NMC811:Super P:PVDF=94:3:3, and dispersed in 1-methyl-2-pyrrolidone (NMP) to form a uniform black slurry. The mixed slurry was coated on both sides of the aluminum foil, and then baked, rolled and cut into pieces to obtain the positive electrode sheet. The compaction density of the positive electrode active material layer was 3.40g / cm 3 ;

[0092] (2) The negative electrode active material graphite (Gr, particle size Dv 50 12μm, particle size Dv 90 The conductive agent acetylene black (Super P), the thickener CMC and the binder SBR are mixed evenly in a mass ratio of AG:Super P:CMC:SBR=96.2:1.2:1.2:1.4, and dispersed in deionized water to form a uniform black slurry. The mixed slurry is coated on both sides of the copper foil, and then baked, rolled and cut into pieces to obtain a negative electrode sheet. The compaction density of the negative electrode sheet is 1.5g / cm 3 ; The film resistivity of the negative electrode sheet is E, in Ω / cm;

[0093] (3) Preparation of electrolyte:

[0094] (3.1) High viscosity organic solvent ethylene carbonate (EC), low viscosity organic solvent ethyl methyl carbonate (EMC) and high viscosity organic solvent diethyl carbonate (DEC) were mixed in a mass ratio of 30:40:30 to form a mixed solvent. Molecular sieve to remove water and set aside;

[0095] (3.2) At room temperature, in a glove box filled with argon, 12.5% ​​of lithium hexafluorophosphate (LFP) in the total mass of the electrolyte was added to the mixed solvent obtained in step (3.1), and the mixture was stirred continuously and cooled to obtain a colorless transparent liquid;

[0096] (3.3) adding 0.2% of vinyl carbonate, 0.5% of vinyl sulfate and 0.5% of lithium difluorophosphate in an amount equivalent to the total mass of the electrolyte to the obtained colorless transparent liquid to obtain the electrolyte;

[0097] (4) The prepared positive electrode sheet, separator (PP separator with a thickness of 14 μm), and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets, and the bare cell is obtained by winding, hot pressing and shaping, and the tabs are welded. The bare cell is placed in an outer packaging aluminum plastic film and baked in an oven at 85±10°C for 24 hours. The prepared electrolyte is injected into the dried battery, allowed to stand, formed, and divided to complete the preparation of the lithium-ion soft-pack battery. The electrolyte injection coefficient is IC, and the unit is g / Ah.

[0098] Example 2

[0099] A secondary battery, the difference from the first embodiment is only in the liquid filling coefficient.

[0100] Example 3

[0101] A secondary battery, the difference from the first embodiment is only in the liquid filling coefficient.

[0102] Example 4

[0103] A secondary battery, the difference from Example 2 is only that the film resistivity of the negative electrode plate is different (different film resistivities can be obtained by adjusting the rolling parameters in the preparation process of the negative electrode plate).

[0104] Example 5

[0105] A secondary battery, the difference from Example 2 is only that the film resistivity of the negative electrode plate is different.

[0106] Example 6

[0107] A secondary battery, the difference from Example 2 is only that the film resistivity of the negative electrode plate is different.

[0108] Example 7

[0109] A secondary battery, which is different from Example 2 only in that in the step (3.1), the mixed solvent is ethylene carbonate, ethyl methyl carbonate, a low-viscosity organic solvent dimethyl carbonate (DMC), and diethyl carbonate prepared in a mass ratio of 30:20:45:5.

[0110] Example 8

[0111] A secondary battery, which is different from Example 2 only in that in the step (3.1), the mixed solvent is ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate prepared in a mass ratio of 20:20:60.

[0112] Example 9

[0113] A secondary battery, which is different from Example 2 only in that in the step (3.1), the mixed solvent is ethylene carbonate, ethyl methyl carbonate, dimethyl carbonate and low-viscosity organic solvent ethyl acetate (EA) prepared in a mass ratio of 20:20:40:20.

[0114] Example 10

[0115] A secondary battery, the only difference from Example 7 is that in the step (3.3), the amount of vinylene carbonate added is 0.1%.

[0116] Embodiment 11

[0117] A secondary battery, the difference from Example 7 is only that in the step (3.3), the amount of vinylene carbonate added is 0.5%.

[0118] Example 12

[0119] A secondary battery, the difference from Example 7 is only that in the step (3.3), the amount of vinylene carbonate added is 1%.

[0120] Example 13

[0121] A secondary battery, the only difference from Example 7 is that in the step (3.3), vinylene carbonate is replaced by fluoroethylene carbonate, and the added amount is 0.1%.

[0122] Embodiment 14

[0123] A secondary battery, the only difference from Example 7 is that in the step (3.3), the amount of vinyl sulfate added is 1%.

[0124] Embodiment 15

[0125] A secondary battery, the only difference from Example 7 is that in the step (3.3), the amount of vinyl sulfate added is 1.5%.

[0126] Example 16

[0127] A secondary battery, the only difference from Example 7 is that in the step (3.3), the amount of vinyl sulfate added is 3%.

[0128] Embodiment 17

[0129] A secondary battery, the only difference from Example 7 is that in step (3.3), vinyl sulfate is replaced by 1,3-propane sultone, and the added amount is 1.5%.

[0130] Embodiment 18

[0131] A secondary battery, the only difference from Example 7 is that in step (3.3), vinyl sulfate is replaced by propenyl-1,3-sultone, and the added amount is 1.5%.

[0132] Embodiment 19

[0133] A secondary battery, the difference from Example 7 is that in step (3.3), vinyl sulfate is replaced by methylene methane disulfonate, and the added amount is 1.5%.

[0134] Embodiment 20

[0135] A secondary battery, the difference from Example 15 is that in the step (3.3), the lithium difluorophosphate is replaced by tris(trimethylsilyl)phosphate, and the added amount is 1%.

[0136] Embodiment 21

[0137] A secondary battery, the only difference from Example 15 is that in the step (3.3), 1% of tris(trimethylsilyl)phosphate is further added.

[0138] Embodiment 22

[0139] A secondary battery, the only difference from Example 15 is that in step (3.3), 1% of tris(trimethylsilyl)phosphate is added, and the added amount of lithium difluorophosphate is 0.9%.

[0140] Embodiment 23

[0141] A secondary battery, the only difference from Example 15 is that in step (3.3), lithium difluorophosphate is replaced by lithium difluorooxalatoborate, and 1% of tris(trimethylsilyl)phosphate is added.

[0142] Embodiments 24 to 29

[0143] A secondary battery, the difference from Example 7 is only that in the step (3.3), the added amounts of vinylene carbonate and vinyl sulfate are different.

[0144] Embodiment 30

[0145] A secondary battery, the difference from Example 1 is only that the particle size D of the negative electrode active material graphite 50 13μm, particle size D 90 It is 18μm.

[0146] Embodiment 31

[0147] A secondary battery, the difference from Example 1 is only that the particle size D of the negative electrode active material graphite 50 12μm, particle size D 90 is 25μm.

[0148] Embodiment 32

[0149] A secondary battery, the difference from Example 1 is only that the particle size D of the negative electrode active material graphite 50 14μm, particle size D 90 It is 18μm.

[0150] Embodiment 33

[0151] A secondary battery, the difference from Example 1 is that the content of vinyl sulfate and lithium difluorophosphate is adjusted to 0.1%.

[0152] Comparative Example 1

[0153] A secondary battery, the difference from the first embodiment is only in the liquid filling coefficient.

[0154] Comparative Example 2

[0155] A secondary battery, which differs from Example 1 in that in the step (3.1), the mixed solvent is ethylene carbonate and ethyl methyl carbonate prepared in a mass ratio of 30:70, and the electrolyte injection coefficient is different.

[0156] Comparative Example 3

[0157] A secondary battery, which differs from Example 1 only in that the film resistivity of the negative electrode plate is different (different film resistivities can be obtained by adjusting the rolling parameters in the preparation process of the negative electrode plate).

[0158] Comparative Example 4

[0159] A secondary battery, which differs from Example 1 in that in the step (3.1), the mixed solvent is ethylene carbonate and ethyl methyl carbonate prepared in a mass ratio of 30:70, and the electrolyte injection coefficient and the film resistivity of the negative electrode plate are different.

[0160] Comparative Example 5

[0161] A secondary battery, which is different from Example 1 only in that in the step (3.1), the mixed solvent is ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate prepared in a mass ratio of 30:10:60.

[0162] Comparative Example 6

[0163] A secondary battery, which is different from Example 1 only in that in the step (3.1), the mixed solvent is ethylene carbonate and ethyl methyl carbonate prepared in a mass ratio of 15:85.

[0164] Comparative Example 7

[0165] A secondary battery, the difference from Example 1 is only that in the step (3.3), ethylene carbonate is not added.

[0166] Comparative Example 8

[0167] A secondary battery, the difference from Example 1 is only that in the step (3.3), vinyl sulfate is not added.

[0168] Comparative Example 9

[0169] A secondary battery, the difference from Example 1 is only that in the step (3.3), lithium difluorophosphate is not added.

[0170] Comparative Example 10

[0171] A secondary battery, which differs from Example 1 only in that the injection coefficient is different and the negative electrode film resistivity is different. In the step (3.1), the mixed solvent is ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate prepared in a mass ratio of 20:20:60; in the step (3.3), fluoroethylene carbonate equivalent to 1% of the total mass of the electrolyte, 3% of vinyl sulfate, 1% of tris(trimethylsilyl) phosphate and 0.9% of lithium difluorophosphate are added to the colorless transparent liquid to obtain the electrolyte.

[0172] The secondary batteries prepared in the above embodiments and comparative examples were tested for performance respectively, and the specific methods are as follows:

[0173] (1) -20°C DCR test: At 25±2°C, the secondary batteries obtained in each embodiment and comparative example were charged at 1C to 4.25V, then discharged at 1C for 30min, adjusted to 50% SOC, and then discharged at 0.36C for 10s after adjusting the temperature to -20°C. The discharge DCR at -20°C was calculated as follows: (voltage change before and after discharge) / discharge current*100%.

[0174] (2) Normal temperature cycle performance test: At 25±2°C, the secondary batteries obtained from each embodiment and comparative example were subjected to charge and discharge cycle test at a charge and discharge rate of 1C / 1C in the range of 2.5 to 4.25V, and the cycle number when the battery capacity retention rate was 80% was recorded. 80 Capacity retention rate (%) = discharge specific capacity corresponding to the last cycle number / discharge specific capacity in the first cycle*100%.

[0175] (3) Battery lithium deposition test method: adjust the temperature to -10°C, charge with a charging current of 0.13C to the upper voltage limit, discharge with a discharging current of 1C to the lower voltage limit, cycle 10 times, adjust the temperature to 25°C, charge with a charging current of 1C to the upper voltage limit, disassemble the battery, and observe whether lithium deposition occurs on the interface. If the area of ​​lithium deposition on the surface of the negative electrode is less than 2%, it is considered that there is no lithium deposition. If the area of ​​lithium deposition on the surface of the negative electrode is greater than or equal to 2% and less than 5%, it is considered that there is slight lithium deposition. If the area of ​​lithium deposition on the surface of the negative electrode is 5-50%, it is considered that there is moderate lithium deposition. If the area of ​​lithium deposition on the surface of the negative electrode is greater than 50%, it is considered that there is severe lithium deposition.

[0176] (4) High-temperature storage gas generation test: The soft-pack batteries obtained in the examples and comparative examples were charged to 4.25V at 1C constant current at 25±2°C, and then charged at 4.25V constant voltage until the current was less than 0.05C, so that they were in a 4.25V fully charged state. The volume of the fully charged battery before storage was tested and recorded as V0; the fully charged battery was then placed in a 60±2°C oven. After 150 days, the battery was taken out and its volume after storage was immediately tested and recorded as V1. The volume expansion rate (%) was calculated as (V1-V0) / V0*100%.

[0177] The test results are shown in Tables 1 to 3, where the setting

[0178] Table 1

[0179]

[0180]

[0181]

[0182] Table 2

[0183]

[0184]

[0185] Table 3

[0186]

[0187]

[0188] From Table 2 we can see that:

[0189] 1) When the secondary battery meets the range requirement of X, the secondary battery has ideal electrochemical performance, its DCR at low temperature can be maintained within the range of 400Ω, and its cycle life at room temperature reaches more than 900 times; on the other hand, the stability and safety of the secondary battery are high, the lithium deposition on the negative electrode surface is good, and the volume expansion rate at high temperature does not exceed 50%.

[0190] 2) According to the data of Examples 1 to 33 and Comparative Example 3, it can be seen that the negative electrode is closely related to the electrolyte. When the membrane resistivity of the negative electrode is in a suitable range, the interface impedance of the secondary battery is small, which can inhibit lithium plating at the negative electrode. When the membrane resistivity of the negative electrode is in a suitable range, the contact efficiency between the negative electrode active material particles in the negative electrode sheet and between the active particles and the binder is high, which has better conduction efficiency for ions and electrons, and is beneficial to improving the cycle life of the secondary battery.

[0191] 3) According to the performance of the secondary batteries prepared in Examples 1 to 33 and Comparative Examples 5 and 6, it can be seen that the viscosity of the solvent in the electrolyte has a great influence on the secondary battery. When the viscosity of the solvent is in an appropriate range, the wettability of the electrolyte can be improved, the lithium ion conduction efficiency can be improved, and the conductivity, cyclability and safety can be improved.

[0192] 4) It can be seen from the products of Examples 1 to 33 and Comparative Examples 7 to 9 that when the three additives in the electrolyte of the present invention are present at the same time, both the fast charge cycle life and the safety performance of the secondary battery can be taken into account.

[0193] 5) It can be seen from Examples 1 to 33 and Comparative Example 10 that the secondary battery of the present invention is constructed based on the overall component relationship. Even if the individual parameters of the individual components meet the range requirements, if the relationship after combination is not considered, the performance of the prepared secondary battery may still not meet the standards.

[0194] 6) As the first additive to ensure fast charging performance and the second additive to ensure safety performance, if the two are maintained in a specific ratio, the overall performance of the product will be better. It can be seen from Examples 7, 10 to 12, and 14 to 16 that the amount of addition of the two directly affects the two performances of the product. Therefore, when the addition amounts of the two are 0.2 to 0.5% and 1 to 1.5% respectively, the product performance is better. According to the comparison between Examples 24 and 27 to 29, it can be seen that even if the total amount of the two additives is the same, if the ratio of the two is maintained within the range of 0.25 to 0.5, the performance of the product can still be maintained better.

[0195] 7) In the negative electrode of the secondary battery, when graphite material is selected as the active material, in addition to the film resistivity, if the particle size Dv is selected 50 and particle size Dv 90When the ratio is between 0.5 and 0.75, the graphite material can better maintain the balance between electrolyte wettability and electronic conductivity, as shown in Example 1 and Examples 30 to 32. The secondary batteries of Example 1 and Example 30 that meet the preferred range have better performance.

Claims

1. A secondary battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the electrolyte comprises a solvent and an additive; the additive comprises a first additive, a second additive and a third additive; the solvent comprises a low-viscosity organic solvent and a high-viscosity organic solvent, wherein the viscosity of the low-viscosity organic solvent is ≤0.7 mPa.s, and the viscosity of the high-viscosity organic solvent is >0.7 mPa.s; The secondary battery meets the following requirements: ; Wherein, the ICg / Ah is the injection coefficient of the electrolyte; The EΩ·cm is the film resistivity of the negative electrode, d=6.70; R is the mass ratio of the low-viscosity organic solvent to the total amount of solvent in the electrolyte; The α is the mass percentage of the first additive in the electrolyte; The β is the mass percentage of the second additive in the electrolyte; The γ is the mass percentage of the third additive in the electrolyte; The first additive includes a carbonate compound; the second additive includes a sulfur-based compound; and the third additive includes a phosphorus-based compound and / or a boron-based compound.

2. The secondary battery according to claim 1, characterized in that: The secondary battery satisfies at least one of the following conditions: (1) 2.30≤IC≤2.80; (2)0.210≤E≤0.253; (3)0.40≤R≤0.80; (4)0.1%≤α≤1.0%; (5)0.1%≤β≤3.0%; (6) 0.1%≤γ≤2%.

3. The secondary battery according to claim 1, characterized in that: The low-viscosity organic solvent includes at least one of dimethyl carbonate, ethyl methyl carbonate, methyl propionate, methyl butyrate, methyl acetate, ethyl acetate, propyl acetate, ethyl butyrate and propyl propionate.

4. The secondary battery according to claim 1, characterized in that: The secondary battery satisfies at least one of the following conditions: (1) The carbonate compound includes at least one of vinylene carbonate, vinyl ethylene carbonate, and fluoroethylene carbonate; (2) The sulfide compound includes at least one of vinyl sulfate, 1,3-propane sultone, propenyl-1,3-sultone, ethylene sulfite, methylene methane disulfonate, and 1,4-butane sultone; (3) The phosphorus-based compound includes at least one of tris(trimethylsilyl)phosphate and lithium difluorophosphate; (4) The boron-based compound includes lithium difluorooxalatoborate.

5. The secondary battery according to claim 1 or 4, characterized in that: The high-viscosity organic solvent includes at least one of ethylene carbonate, propylene carbonate, butylene carbonate, diethyl carbonate, methylpropyl carbonate, diphenyl carbonate, and γ-butyrolactone.

6. The secondary battery according to claim 1, characterized in that: The high-viscosity organic solvent includes at least one of ethylene carbonate, propylene carbonate, and diethyl carbonate, and the low-viscosity organic solvent includes ethyl methyl carbonate and / or ethyl acetate.

7. The secondary battery according to claim 1, characterized in that: The α:β=0.25~0.

5.

8. The secondary battery according to claim 1, characterized in that: The negative electrode sheet contains a negative electrode active material, and the negative electrode active material includes a graphite material, and the particle size Dv of the graphite material is 50 The particle size Dv of the graphite material 90 The ratio is 0.5~0.75; among them, Dv 50 Dv is the particle size corresponding to the volume cumulative distribution percentage of the graphite material reaching 50%, 90 It is the particle size corresponding to when the volume cumulative distribution percentage of the graphite material reaches 90%.

9. The secondary battery according to claim 8, characterized in that: The particle size Dv of the graphite material 50 ≤15μm, the particle size Dv of the graphite material 90 ≤25μm.

10. An electrical device, characterized in that: It comprises the secondary battery according to any one of claims 1 to 9, wherein the secondary battery is used as a power supply for the electrical device.