Pyrrole nitrogen-doped carbon shell coated Fe prepared by a microfluidic method 3 C core nanosphere catalyst and its preparation method and application
The pyrrole nitrogen-doped carbon shell coated Fe3C core nanosphere catalyst prepared by microfluidic control method solves the problems of sintering of iron-based catalysts and wide distribution of products in Fischer-Tropsch synthesis, realizing the stability and product selectivity of the catalyst. Improvement significantly improves the performance of Fischer Tropsch synthesis.
Patent Information
- Application Number
- CN202311757201.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-12-19
AI Technical Summary
Iron-based catalysts are prone to sintering, agglomeration and wide distribution of products during Fischer-Tropsch synthesis, resulting in a reduced catalytic activity and limiting their application in the FTS process.
A pyrrole nitrogen-doped carbon shell coated Fe3C core nanosphere catalyst was prepared by microfluidic control method. Through the microfluidic coprecipitation reaction and calcination steps, a single catalyst with stable structure and physical phase composition was formed.
It improves the stability of the catalyst, prevents sintering and agglomeration, promotes the electron reaction of Fe-C, enhances the reaction activity and regulates the selective formation of heavy olefins of products, and significantly improves the catalytic performance of Fischer-Tropsch synthesis.
Smart Images

Figure CN117753454B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst prepared by a microfluidic method, and a preparation method and application thereof. Background Art
[0002] With the rapid economic development and accelerated industrialization, people's demand for liquid fuels and high-value-added chemicals has increased, resulting in the uncontrolled exploitation of limited oil resources and more serious environmental problems. my country's energy distribution is characterized by "rich in coal, less oil, and poor in gas". The strategy of indirectly liquefying carbon-containing resources such as coal, natural gas, and biomass into clean liquid fuels and fine chemicals using Fischer-Tropsch synthesis technology is of great significance to my country's energy utilization and environmental protection.
[0003] In the Fischer-Tropsch synthesis process, iron-based catalysts have attracted much attention from academia and industry due to their low price, wide operating conditions, rich and adjustable product variety, and high activity. However, iron-based catalysts are prone to phase change, sintering, and carbon deposition during the FTS process, leading to deactivation. In addition, due to the wide distribution of their products (C1-C 50 ), which limits the application of iron-based catalysts in the FTS process. 5+ = It is an ideal chemical intermediate for a large number of high value-added chemicals. However, there are few research methods for directly converting syngas into heavy olefins, most of which focus on light olefins or C 5+ Therefore, it is still necessary to develop, design and optimize iron-based catalysts, study the complex evolution of iron species during the reaction, understand the mechanism of the reaction active center and the influence of catalyst structure on performance, improve reaction activity and regulate product selectivity to generate heavy olefins.
[0004] The phase composition of iron-based catalysts is complex and diverse, and different phases can also transform into each other, which hinders the exploration of the relationship between the iron phase and the activity of the Fischer-Tropsch synthesis reaction. Although iron carbide is the active phase determined by the Fischer-Tropsch synthesis reaction, it is still difficult to reveal their intrinsic catalytic principles in the reaction process due to the interference of other iron-containing substances. In addition, due to the intense heat release of iron-based catalysts during the reaction, sintering and agglomeration are prone to occur, resulting in reduced catalytic activity, which hinders the application of iron-based catalysts in Fischer-Tropsch synthesis. Therefore, how to obtain iron-based catalysts with stable structure and single phase composition and regulate the product to produce heavy olefins is of great significance to the development of efficient iron-based catalysts for Fischer-Tropsch synthesis. Summary of the invention
[0005] The main purpose of the present invention is to propose a pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst prepared by a microfluidic method and its preparation method and application, aiming to solve the problems of existing iron-based catalysts being prone to sintering, agglomeration and wide distribution of products in the Fischer-Tropsch synthesis reaction.
[0006] To achieve the above object, the present invention proposes a pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst prepared by a microfluidic method. The nanosphere catalyst has a single-phase Fe3C core and is coated with pyrrole nitrogen-doped carbon on the surface.
[0007] The present invention also provides a method for preparing the pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst as described above, comprising the following steps:
[0008] S1, mixing polyvinyl pyrrolidone and a precursor salt to obtain a solution A, and dissolving ferrocyanide in water to obtain a solution B;
[0009] S2, subjecting the solution A and the solution B to a microfluidic coprecipitation reaction, followed by aging, centrifugation, washing, and drying to obtain a PB precursor;
[0010] S3, grinding, granulating and calcining the PB precursor to obtain a pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst.
[0011] Optionally, in step S1, the precursor salt is any one of FeCl3, FeSO4, Fe(NO3)3, FeCl2, Fe(C2H3O2)3, Fe2(C2O4)3; and / or,
[0012] The ferrocyanide is any one of Na4[Fe(CN)6], K3[Fe(CN)6], K4[Fe(CN)6], and Na3[Fe(CN)6]; and / or,
[0013] The water includes deionized water.
[0014] Optionally, in step S1, the molar ratio of the precursor salt to ferrocyanide is 5-15:9-20.
[0015] Optionally, in step S2, the temperature of the microfluidic co-precipitation reaction is 35-90°C.
[0016] Optionally, in step S2, the microfluidic coprecipitation reaction uses a microchannel reactor; and / or,
[0017] The flow rates of the two pumps of the microchannel reactor are both 4-50 ml / min.
[0018] Optionally, in step S2, the aging time is 12 to 48 hours; and / or,
[0019] The centrifugal speed is 7000-12000 rpm; and / or,
[0020] The centrifugation time is 5 to 30 minutes.
[0021] Optionally, in step S2, the drying temperature is 60-120° C.; and / or,
[0022] The drying time is 12 to 48 hours.
[0023] Optionally, in step S3, the calcination temperature is 450-750° C.; and / or,
[0024] The calcination time is 60 to 600 minutes.
[0025] The present invention also proposes an application of a pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst prepared by the microfluidic method as described above.
[0026] The beneficial effects of the present invention are:
[0027] (1) The pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst prepared by the microfluidic method provided by the present invention has a pyrrole nitrogen-doped carbon shell, which can not only improve the stability of the catalyst and prevent sintering and agglomeration, but also provide electrons for Fe-C, promote carbon-carbon coupling while inhibiting catalytic hydrogenation, improve the reaction activity while regulating the product to selectively generate heavy olefins. The nanosphere catalyst has a novel structure, excellent syngas catalytic performance, a single phase composition, and promotes the Fischer-Tropsch synthesis reaction.
[0028] (2) The present invention utilizes a microfluidic co-precipitation method to synthesize a core-shell structured pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere. By controlling the microfluidic reaction conditions, single-phase stable iron carbide particles are obtained after calcination for Fischer-Tropsch synthesis of high-efficiency liquid fuels and fine chemicals, and have excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 is a SEM image of the catalyst obtained in Example 1 of the present invention;
[0031] Figure 2 is the XRD pattern of the catalyst obtained in Example 1 of the present invention;
[0032] Figure 3 This is the full XPS spectrum of the catalyst obtained in Example 1 of the present invention;
[0033] Figure 4 This is the N1s spectrum of the XPS of the catalyst obtained in Example 1 of the present invention.
[0034] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0035] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0036] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0037] Example 1 Preparation method of pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst
[0038] (1) Preparation of precursor solution: 3 g PVP was slowly added into 50 ml deionized water stirred at 450 rpm, and stirred for 30 min to obtain a clear solution. Then, 0.009 mol FeCl3 was added into the clear solution and stirred for 30 min to obtain solution A. 0.0135 mol Na4[Fe(CN)6] was added into a beaker containing 100 ml deionized water stirred at 450 rpm, and stirred for 30 min to obtain a clear solution B.
[0039] (2) Microfluidic coprecipitation reaction: Heat solutions A and B to 50°C, place the three-way pipe of the microchannel reactor in an oil bath for insulation treatment, ensure that the pipe temperature is also maintained at 50°C during the reaction, turn on the Hastelloy pump and the stainless steel pump to extract solutions A and B respectively, set the flow rate of the two pumps to 5ml / min, introduce solutions A and B into another beaker C through the microfluidic channel, maintain the temperature of beaker C at 50°C, and stir the solution for 60 minutes after the addition is completed. Stand still and age in the dark for 24 hours, centrifuge at 8500rpm for 5 minutes, wash with deionized water and anhydrous ethanol three times, and then put it in a vacuum drying oven at 60°C for 24 hours.
[0040] (3) Heat treatment: The dried solid was ground into powder and pressed into tablets to obtain a 30-mesh catalyst. 5 g of the catalyst was placed in a quartz tube and heated to 550 °C at 5 °C / min under a N2 atmosphere and maintained for 1 h to obtain a pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst.
[0041] Example 2 Preparation method of pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst
[0042] (1) Preparation of precursor solution: 4 g PVP was slowly added into 50 ml deionized water stirred at 450 rpm. After stirring for 30 min, a clear solution was obtained. Then, 0.005 mol FeSO4 was added into the clear solution and stirred for 30 min to obtain solution A. 0.009 mol Na4[Fe(CN)6] was added into a beaker containing 100 ml deionized water stirred at 450 rpm and stirred for 30 min to obtain a clear solution B.
[0043] (2) Microfluidic coprecipitation reaction: Heat solutions A and B to 35°C, place the three-way pipe of the microchannel reactor in an oil bath for insulation treatment, ensure that the pipe temperature is also maintained at 35°C during the reaction, turn on the Hastelloy pump and the stainless steel pump to extract solutions A and B respectively, set the flow rate of the two pumps to 5ml / min, introduce solutions A and B into another beaker C through the microfluidic channel, maintain the temperature of beaker C at 35°C, and stir the solution for 60 minutes after the addition is completed. Stand still and age in the dark for 12 hours, centrifuge at 7000rpm for 10 minutes, wash with deionized water and anhydrous ethanol three times, and then put it in a vacuum drying oven at 90°C for 12 hours.
[0044] (3) Heat treatment: The dried solid was ground into powder and pressed into tablets to obtain a 20-mesh catalyst. 5 g of the catalyst was placed in a quartz tube and heated to 450 °C at 5 °C / min under a N2 atmosphere and maintained for 6 h to obtain a pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst.
[0045] Example 3 Preparation method of pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst
[0046] (1) Preparation of precursor solution: 5 g PVP was slowly added into 50 ml deionized water stirred at 450 rpm, and stirred for 30 min to obtain a clear solution. Then, 0.015 mol FeCl3 was added into the clear solution and stirred for 30 min to obtain solution A. 0.02 mol K3[Fe(CN)6] was added into a beaker containing 100 ml deionized water stirred at 450 rpm, and stirred for 30 min to obtain a clear solution B.
[0047] (2) Microfluidic coprecipitation reaction: Heat solutions A and B to 90°C, place the three-way pipe of the microchannel reactor in an oil bath for insulation treatment, ensure that the pipe temperature is also maintained at 90°C during the reaction, turn on the Hastelloy pump and the stainless steel pump to extract solutions A and B respectively, set the flow rate of the two pumps to 5ml / min, introduce solutions A and B into another beaker C through the microfluidic channel, maintain the temperature of beaker C at 90°C, and stir the solution for 60 minutes after the addition is completed. Stand still and age in the dark for 48 hours, centrifuge at 12000rpm for 30 minutes, wash with deionized water and anhydrous ethanol three times, and then put it in a vacuum drying oven at 120°C for 48 hours.
[0048] (3) Heat treatment: The dried solid was ground into powder and pressed into tablets to obtain a 40-mesh catalyst. 5 g of the catalyst was placed in a quartz tube and heated to 750 °C at 5 °C / min under a N2 atmosphere and maintained for 10 h to obtain a pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst.
[0049] Comparative Example 1 Preparation method of Fe3C catalyst
[0050] (1) Preparation of precursor solution: 0.009 mol FeCl3 was added to the clear solution and stirred for 30 min to obtain solution A; 0.0135 mol Na4[Fe(CN)6] was added to a beaker containing 100 ml deionized water stirred at 450 rpm and stirred for 30 min to obtain a clear solution B.
[0051] (2) Microfluidic coprecipitation reaction: Heat solutions A and B to 50°C, place the three-way pipe of the microchannel reactor in an oil bath for insulation treatment, ensure that the pipe temperature is also maintained at 50°C during the reaction, turn on the Hastelloy pump and the stainless steel pump to extract solutions A and B respectively, set the flow rate of the two pumps to 5ml / min, introduce solutions A and B into another beaker C through the microfluidic channel, maintain the temperature of beaker C at 50°C, and stir the solution for 60 minutes after the addition is completed. Stand still and age in the dark for 24 hours, centrifuge at 8500rpm for 5 minutes, wash with deionized water and anhydrous ethanol three times, and then put it in a vacuum drying oven at 60°C for 24 hours.
[0052] (3) Heat treatment: The dried solid was ground into powder and pressed into tablets to obtain a 30-mesh catalyst. 5 g of the catalyst was placed in a quartz tube and heated to 550°C at 5°C / min under a N2 atmosphere and maintained for 1 h to obtain a Fe3C catalyst.
[0053] Comparative Example 2 Preparation method of Fe3C catalyst
[0054] (1) Preparation of precursor solution: 3 g of PVP was slowly added into 50 ml of deionized water stirred at 450 rpm. After stirring for 30 min to obtain a clear solution, 0.009 mol of FeCl3 was added into the clear solution and stirred for 30 min to obtain solution A.
[0055] (2) Microfluidic reaction: Heat solution A to 50°C, place the three-way pipe of the microchannel reactor in an oil bath for insulation treatment, ensure that the pipe temperature is also maintained at 50°C during the reaction, turn on the Hastelloy pump to extract solution A, set the pump flow rate to 5ml / min, introduce solution A into another beaker C through the microfluidic channel, maintain the temperature of beaker C at 50°C, and stir the solution for 60 minutes after the addition is completed. Stand still and age in the dark for 24 hours, centrifuge at 8500rpm for 5 minutes, wash with deionized water and anhydrous ethanol three times, and then put it into a vacuum drying oven at 60°C for 24 hours.
[0056] (3) Heat treatment: The dried solid was ground into powder and pressed into tablets to obtain a 30-mesh catalyst. 5 g of the catalyst was placed in a quartz tube and heated to 550°C at 5°C / min under a N2 atmosphere and maintained for 1 h to obtain a Fe3C catalyst.
[0057] Comparative Example 3 Preparation method of Fe3C catalyst
[0058] (1) Preparation of precursor solution: 3 g PVP was slowly added into 50 ml deionized water stirred at 450 rpm, and stirred for 30 min to obtain a clear solution. Then, 0.009 mol FeCl3 was added into the clear solution and stirred for 30 min to obtain solution A. 0.0135 mol Na4[Fe(CN)6] was added into a beaker containing 100 ml deionized water stirred at 450 rpm, and stirred for 30 min to obtain a clear solution B.
[0059] (2) Hydrothermal reaction: Solutions A and B were mixed and heated to 50°C, transferred to a hydrothermal reactor, placed in an oven at 110°C for reaction for 24 h, washed with deionized water and anhydrous ethanol three times, respectively, and then placed in a vacuum drying oven at 60°C for drying for 24 h.
[0060] (3) Heat treatment: The dried solid was ground into powder and pressed into tablets to obtain a 30-mesh catalyst. 5 g of the catalyst was placed in a quartz tube and heated to 550°C at 5°C / min under a N2 atmosphere and maintained for 1 h to obtain a Fe3C catalyst.
[0061] Test methods and results
[0062] The pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst obtained in Example 1 was observed using a scanning electron microscope. Figure 1 The pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst obtained in Example 1 was detected by X-ray diffractometer to obtain Figure 2 The pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst obtained in Example 1 was detected by X-ray photoelectron spectrometer to obtain Figure 3 The pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst obtained in Example 1 was subjected to N1s spectrum analysis to obtain Figure 4 The catalysts prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to a performance test for the synthesis of long-chain olefins from syngas. The specific test method is as follows: 0.2 g of the prepared catalyst was loaded into a fixed bed reactor. The reaction conditions were 300° C., H2 / CO=1 (molar ratio), 2 MPa, 6000 h -1 , Fischer-Tropsch synthesis reaction was carried out, and the specific test results are shown in Table 1.
[0063] Table 1 Performance test of catalysts for synthesis gas to long-chain olefins
[0064]
[0065] Depend on Figure 1 It can be seen that the catalyst provided in the embodiment of the present invention is a nano-scale granular spherical substance; Figure 2It can be seen that the catalyst provided by the embodiment of the present invention has a high crystallinity and is a single phase crystal; Figure 3 Obvious C and N peaks can be clearly observed, indicating that there are nitrogen and carbon on the catalyst surface, indicating that the nitrogen-doped carbon shell was successfully prepared; Figure 4 The N1s spectrum of the catalyst provided in the embodiment of the present invention attributes the binding energies of about 398.5 eV, 399.8 eV and 401.1 eV to pyridine N, pyrrole N and graphite N, respectively, indicating that the catalyst wrapped in the pyrrole nitrogen-doped carbon shell is successfully prepared; as can be seen from Table 1, compared with the low CO conversion rate of the catalyst provided in Comparative Examples 1 to 3, which is lower than 60%, the CO conversion rate of the catalyst provided in Examples 1 to 3 of the present invention is higher, which is higher than 70%, and the high-value product C in Examples 1 to 3 of the present invention is 5+ = The selectivity of by-product CH4 is higher than the comparative ratio, and the selectivity of by-product CH4 is lower than the comparative ratio.
[0066] In summary, the pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst prepared by the microfluidic method provided by the present invention has a single phase composition and a novel structure. It is used for Fischer-Tropsch synthesis to produce high-efficiency liquid fuels and fine chemicals, and has excellent performance, high conversion rate, and better gas product selectivity.
[0067] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst prepared by a microfluidic method, characterized in that: The nanosphere catalyst has a single-phase Fe3C core and is coated with pyrrole nitrogen-doped carbon on the surface; The preparation method of the pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst comprises the following steps: S1, mixing polyvinyl pyrrolidone and a precursor salt to obtain a solution A, and dissolving ferrocyanide in water to obtain a solution B; S2, subjecting the solution A and the solution B to a microfluidic coprecipitation reaction, followed by aging, centrifugation, washing, and drying to obtain a PB precursor; S3, grinding, granulating and calcining the PB precursor to obtain a pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst; The precursor salt is any one of FeCl3, FeSO4, Fe(NO3)3, FeCl2, Fe(C2H3O2)3, and Fe2(C2O4)3.
2. The pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst according to claim 1, characterized in that: In step S1, the ferrocyanide is any one of Na4[Fe(CN)6], K3[Fe(CN)6], K4[Fe(CN)6], and Na3[Fe(CN)6]; The water includes deionized water.
3. The pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst according to claim 1, characterized in that: In step S1, the molar ratio of the precursor salt to ferrocyanide is 5-15:9-20.
4. The pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst according to claim 1, characterized in that: In step S2, the temperature of the microfluidic coprecipitation reaction is 35-90°C.
5. The method for preparing the pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst according to claim 1, characterized in that: In step S2, the microfluidic coprecipitation reaction uses a microchannel reactor; The flow rates of the two pumps of the microchannel reactor are both 4-50 ml / min.
6. The pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst according to claim 1, characterized in that: In step S2, the aging time is 12 to 48 hours; The centrifugal speed is 7000-12000 rpm; The centrifugation time is 5 to 30 minutes.
7. The pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst according to claim 1, characterized in that: In step S2, the drying temperature is 60-120°C; The drying time is 12 to 48 hours.
8. The pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst according to claim 1, characterized in that: In step S3, the calcination temperature is 450-750°C; The calcination time is 60 to 600 minutes.
9. An application of the pyrrole nitrogen-doped carbon shell-coated Fe3C core nanosphere catalyst prepared by the microfluidic method as claimed in claim 1 for Fischer-Tropsch synthesis reaction.
Citation Information
Patent Citations
Carbon coated iron and iron carbide nano-composite material and preparation method thereof
CN109305684A
High-activity metastable-state iron carbide catalyst as well as preparation method and application thereof
CN116099559A
Preparation of Iron / Carbon Nanocomposite Catalysts for Fischer-Tropsch Synthesis Reaction and Related Production of Liquid Hydrocarbons
US20130341242A1
Cited By
Methanol catalyst for improving sulfur tolerance and preparation method thereof