A defect-controlled two-dimensional material heterojunction device and its preparation method and application

By creating defects on the surface of two-dimensional materials and growing porous skeleton structures, the difficulty of selective design of two-dimensional materials heterojunction devices is solved, high selectivity and large-area preparation are achieved, and it is suitable for a variety of electronic devices.

CN117907410BActive Publication Date: 2024-11-26SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311818080.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2024-11-26
Estimated Expiration
2043-12-27

Smart Images

  • Figure CN117907410B_ABST
    Figure CN117907410B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of electronic devices, and specifically relates to a defect-regulated two-dimensional material heterojunction device and its preparation method and application, including the following steps: transferring a two-dimensional material to a substrate, and preparing an electrode to form a two-dimensional material device; making defects on the surface of the two-dimensional material by plasma cleaning; immersing the defective two-dimensional material device in a low-temperature metal ion solution; immersing the immersed two-dimensional material device in a ligand solution again, and cyclically immersing, growing a second layer of porous skeleton structure material on the surface of the two-dimensional material to form a heterojunction; cleaning and drying to obtain a defect-regulated two-dimensional material heterojunction device. Compared with the prior art, the present invention solves the problem that the prior art cannot be selectively designed; this scheme realizes a two-dimensional material heterojunction device with target sites and directional selectivity by anchoring metal ions with defects, and the preparation method is simple and controllable, and can be prepared on a large area.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of electronic devices, and specifically relates to a defect-regulated two-dimensional material heterojunction device and a preparation method and application thereof. Background Art

[0002] Due to the limited sensitivity, low selectivity and poor stability of traditional sensing materials, it is difficult to break through the performance bottleneck of existing electronic devices under traditional sensing material systems. In order to break through these performance bottlenecks, researchers are exploring new sensing material systems, such as two-dimensional materials, nanomaterials, organic-inorganic hybrid materials, etc.

[0003] Among them, two-dimensional quantum materials with atomic-level thickness have many novel electronic properties and are the core foundation for the performance transformation of electronic devices such as sensors, batteries, and capacitors. At present, many international scholars have done a lot of exploration in the research of two-dimensional materials for electronic devices, but the scale that can be achieved by the manufacturing process is small, and the lack of sensor selectivity has not been solved, making it difficult to apply to actual large-scale applications. For example, Samsung combines two layers of metal chalcogenide-based materials (two-dimensional material elements and semiconductor devices, CN104617135A), composites graphene and metal chalcogenide-based materials (including metal-two-dimensional material-semiconductor contact semiconductor devices, CN106169502A), and Intel loads two-dimensional materials on flexible substrates such as organic electronic devices or polymer electronic devices. However, the preparation of these electrode devices still does not solve the directional selectivity design.

[0004] Therefore, it is necessary to develop a method that is simple, highly controllable, and can be used to prepare two-dimensional material heterojunction devices with target sites and directional selectivity over a large area. Summary of the invention

[0005] The purpose of the present invention is to solve at least one of the above problems and to provide a defect-regulated two-dimensional material heterojunction device and its preparation method and application, so as to solve the problem that selective design is not possible in the prior art; this scheme realizes a two-dimensional material heterojunction device with target sites and directional selectivity by anchoring metal ions with defects, and the preparation method is simple and controllable, and can be prepared on a large area.

[0006] The purpose of the present invention is achieved through the following technical solutions:

[0007] The first aspect of the present invention discloses a method for preparing a defect-controlled two-dimensional material heterojunction device, comprising the following steps:

[0008] S1: Transfer the two-dimensional material to the substrate and prepare electrodes to form a two-dimensional material device;

[0009] S2: Creating defects on the surface of 2D materials by plasma cleaning;

[0010] S3: immersing the defective two-dimensional material device in a low-temperature metal ion solution;

[0011] S4: immersing the immersed two-dimensional material device in the ligand solution again, and cyclically immersing the device to grow a second layer of porous skeleton structure material on the surface of the two-dimensional material to form a heterojunction;

[0012] S5: Clean and dry to obtain a defect-regulated two-dimensional material heterojunction device.

[0013] Preferably, in step S1, the two-dimensional material is a single-layer graphene, a multi-layer graphene, a single-layer metal chalcogenide, a multi-layer metal chalcogenide, a single-layer hexagonal boron nitride or a multi-layer hexagonal boron nitride; the substrate is Si / SiO2, polyester resin, polyethylene oxide, polyimide or sapphire, and the surface roughness of the substrate is less than 100nm; the electrode is a metal electrode, and the metal is one or more of Al, Ni, Mo, Cu, Au, Ti, Cr, Nb, Ag, Pt and Pd, and the electrode thickness is less than 200nm.

[0014] Preferably, in step S1, the two-dimensional material is grown on the substrate by chemical vapor deposition; and the electrode is prepared by vacuum evaporation or magnetron sputtering.

[0015] Preferably, in step S2, the plasma cleaning has a power of 10 to 1000 W, an atmosphere of one or more of argon, nitrogen, oxygen, ammonia and hydrogen sulfide, a gas flow rate of 10 to 1000 sccm, and a cleaning time of 1 to 10 min.

[0016] Preferably, in step S3, the low-temperature metal ion solution: the temperature is -40 to 5°C, the solute is one or more of gold acetate, platinum acetate, silver acetate, palladium acetate, zinc acetate, cobalt acetate, copper acetate, manganese acetate, gold chlorate, platinum chlorate, silver chlorate, palladium chlorate, zinc chloride, cobalt chloride, copper chloride, manganese chloride, gold acetylacetonate, platinum acetylacetonate, silver acetylacetonate and palladium acetylacetonate, the solvent is one or more of ultrapure water, ethanol, methanol and isopropanol, the concentration of the solution is 1 μM to 10 mM; the immersion time is 1 to 60 min.

[0017] Preferably, in step S4, the ligand solution: the solute is one or more of imidazole derivatives, triphenylene derivatives, triazole derivatives and trimesic acid derivatives, the solvent is one or more of ultrapure water, ethanol, methanol and isopropanol, the concentration of the solution is 1 μM to 10 mM; the immersion time is 1 to 60 min, and the number of repetitions is 2 to 10 times.

[0018] Preferably, in step S5, the cleaning solvent is one or more of ultrapure water, ethanol, methanol and isopropanol; the drying includes freeze-drying and oven-drying: when freeze-drying is adopted, the freeze-drying temperature is -10 to -60°C, and when oven-drying is adopted, the oven-drying temperature is 50 to 100°C.

[0019] The second aspect of the present invention discloses a defect-regulated two-dimensional material heterojunction device, which is prepared by any of the methods described above.

[0020] The third aspect of the present invention discloses an application of the defect-regulated two-dimensional material heterojunction device as described above in an electronic device.

[0021] Preferably, the electronic device includes a gas sensor, a liquid sensor, a photodetector, a flexible sensor, an electrode of a lithium battery, an electrode of a fuel cell, an electrode of a supercapacitor and a light-emitting device.

[0022] The working principle of the present invention is:

[0023] First, the two-dimensional material grown by chemical vapor deposition has a single-layer or few-layer structure with strong surface controllability; further, a plasma cleaning method is used to implement plasma defect engineering, and the surface of the first layer of two-dimensional material transferred to the substrate is etched to obtain a large number of defects; using these defects, metal ions can be anchored by chelation, and the aggregation / Ostwald ripening effect of metals can be prevented at low temperatures to form nanoparticles, ensuring abundant coordination sites; further, in the ligand solution, through the action of click chemistry ligands, a second layer of porous skeleton structure material is grown at the defects of the first layer of two-dimensional material to form a heterojunction, and this step is repeated many times to allow the second layer of porous skeleton structure to grow completely; finally, the unreacted metal or ligand is cleaned off to obtain the final two-dimensional material heterostructure device.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The defect-regulated two-dimensional material heterojunction device of the present invention comprises a first layer of two-dimensional material and a second layer of porous skeleton structure material grown on the surface thereof. It has a simple structure and adjustable components and can be used for the directional design of devices with high selectivity and high activity.

[0026] 2. The defect-regulated two-dimensional material heterojunction device of the present invention utilizes the etching effect of plasma on the surface of the first layer structure to achieve defect regulation, providing a site basis for the preparation of the second layer porous skeleton structure. At the same time, the growth of the second layer porous skeleton structure material can stably synthesize the second layer porous skeleton structure and form a specific pore structure through the click chemistry of the ligand, providing a rich structure for the interface.

[0027] 3. The two-dimensional material heterojunction device of the present invention can be applied to energy, environment, semiconductor fields such as sensors (such as gas sensors, liquid sensors, photodetectors, flexible sensors), lithium-sulfur batteries, lithium-air batteries, fuel cells, supercapacitors, lithium battery negative electrode materials and light-emitting devices, and has a wide range of uses. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A schematic diagram of the structure of a defect-regulated two-dimensional material heterojunction device of the present invention;

[0029] Figure 2 This is an optical micrograph of the Cu3HHTP2 / single-layer molybdenum disulfide device of Example 2;

[0030] Figure 3 The gas sensing performance test of the Cu3HHTP2 / monolayer molybdenum disulfide device of Example 2;

[0031] Figure 4 An optical micrograph of a Cu3HHTP2 / single-layer MoS2 device of a comparative example;

[0032] Figure 5 The gas sensing performance test of the Cu3HHTP2 / single-layer molybdenum disulfide device for comparison example. DETAILED DESCRIPTION

[0033] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0034] In the following description, unless otherwise specified, the reagents used are conventional commercially available products, and the methods used are well known in the art.

[0035] like Figure 1 As shown, the defect-regulated two-dimensional material heterojunction device: a first layer of two-dimensional material is deposited on a substrate by chemical vapor deposition, and then an electrode is prepared; defects are formed in the first layer of two-dimensional material by plasma cleaning, and then it is immersed in a low-temperature metal ion solution for soaking; the immersed two-dimensional material device is immersed in a ligand solution again, and the soaking cycle is repeated for multiple times to complete the growth of the second layer of porous skeleton structure material; finally, it is washed with a solvent and dried to obtain.

[0036] More specifically,

[0037] A defect-controlled two-dimensional material heterojunction device preparation method and application, comprising the following specific steps:

[0038] (1) transferring the two-dimensional material grown by chemical vapor deposition onto a target substrate and preparing electrodes to form a two-dimensional material device;

[0039] (2) Cleaning the surface of the two-dimensional material by plasma cleaning to create defects;

[0040] (3) placing the defective two-dimensional material into a low-temperature metal ion solution;

[0041] (4) further immersing in the ligand solution for multiple immersion cycles to complete the growth of the second layer of porous skeleton structure material;

[0042] (5) Wash the sample surface with a solvent to remove residual reactants and then dry it.

[0043] Wherein, the two-dimensional material grown by the chemical vapor deposition method described in step 1 includes any one of single-layer / multi-layer graphene, single-layer / multi-layer metal chalcogenide, and single-layer / multi-layer hexagonal boron nitride.

[0044] Wherein, the target substrate described in step (1) comprises any one of Si / SiO2, polyester resin, polyethylene oxide, polyimide, and sapphire, and the surface roughness is less than 100 nm, and the metal electrode is prepared on the surface by vacuum evaporation or magnetron sputtering patterning, and the metal comprises any one of Al, Ni, Mo, Cu, Au, Ti, Cr, Nb, Ag, Pt, and Pd or a combination of at least two thereof, and the electrode thickness is less than 200 nm;

[0045] The power of the plasma cleaning in step (2) is 10 to 1000 W, the atmosphere is any one of argon, nitrogen, oxygen, ammonia, and hydrogen sulfide, or a combination of at least two of them, the gas flow rate is 10 to 1000 sccm, and the cleaning time is 1 to 10 min.

[0046] The temperature of the low-temperature metal ion solution in step (3) is between -40 and 5°C, the solute is any one of gold acetate, platinum acetate, silver acetate, palladium acetate, zinc acetate, cobalt acetate, copper acetate, manganese acetate, gold chlorate, platinum chlorate, silver chlorate, palladium chlorate, zinc chloride, cobalt chloride, copper chloride, manganese chloride, gold acetylacetonate, platinum acetylacetonate, silver acetylacetonate, and palladium acetylacetonate, or a combination of at least two thereof; the solvent is any one of ultrapure water, ethanol, methanol, and isopropanol, or a combination of at least two thereof; the solution concentration is between 1 μM and 10 mM; and the immersion time is between 1 and 60 min;

[0047] Wherein, the solute of the ligand solution in step (4) is any one or a combination of at least two of imidazole derivatives, triphenylene derivatives, triazole derivatives and trimesic acid derivatives, the solvent is any one or a combination of at least two of ultrapure water, ethanol, methanol and isopropanol, the concentration is 1 μM to 10 mM, the immersion time is 1 to 60 min, and the number of repetitions is 2 to 10 times;

[0048] The solvent used for surface cleaning in step (5) is any one of ultrapure water, ethanol, methanol, isopropanol, or a combination of at least two thereof, and the drying method includes freeze-drying and drying, the freeze-drying temperature is -10 to -60°C, and the drying temperature is 50 to 100°C.

[0049] An application of a defect-regulated two-dimensional material heterojunction device, including heterojunction electrodes used as gas sensors, liquid sensors, photodetectors, flexible sensors, electrodes of lithium batteries (such as lithium-sulfur batteries, lithium-air batteries, lithium batteries), electrodes of fuel cells, electrodes of supercapacitors, and light-emitting devices.

[0050] Example 1

[0051] (1) Transferring the single-layer graphene grown by chemical vapor deposition onto a Si / SiO2 substrate, and preparing a 50 nm thick Au electrode by vacuum evaporation to form a single-layer graphene device;

[0052] (2) Cleaning the surface of the monolayer graphene by 10W plasma cleaning for 1 min in an Ar atmosphere to create defects;

[0053] (3) placing the defective single-layer graphene device in a methanol solution containing 1 mM zinc chloride at -5°C for 10 min;

[0054] (4) The single-layer graphene device was immersed in a methanol solution containing 4 mM 2-methylimidazole for 10 min, and the immersion cycle was repeated three times to complete the growth of the second layer of porous framework structure ZIF-8;

[0055] (5) The sample surface was washed with methanol solvent to remove residual reactants and dried at 60 °C to obtain a ZIF-8 / single-layer graphene device.

[0056] The device was tested on an electrochemical workstation and the resistance was about 1 kΩ under the cyclic voltammetry test conditions of -1 to 1 V. The device was placed in a test gas chamber, 1 V voltage was applied, and 1 to 10 ppm concentration of toluene was introduced, which enabled the sensing of toluene gas.

[0057] Example 2

[0058] (1) Transferring a monolayer of MoS2 grown by chemical vapor deposition onto a Si / SiO2 substrate, and preparing a 5 nm thick Ti and a 50 nm thick Au electrode by vacuum evaporation to form a monolayer MoS2 device;

[0059] (2) Clean the surface of the monolayer MoS2 by 50W plasma cleaning for 2 min in N2 atmosphere to create defects;

[0060] (3) placing the defective monolayer MoS2 device in a -10°C ethanol solution containing 1 mM copper acetate for 20 min;

[0061] (4) The monolayer MoS2 device was immersed in an ethanol solution containing 1 mM 2,3,6,7,10,11-hexahydroxytriphenylene for 20 min, and the immersion cycle was repeated three times to complete the growth of the second layer of the porous framework structure Cu3HHTP2;

[0062] (5) The sample surface was washed with ethanol solvent to remove residual reactants and dried at 60°C to obtain a Cu3HHTP2 / single-layer MoS2 device.

[0063] The device was tested on an electrochemical workstation and the resistance was about 10kΩ under the cyclic voltammetry test conditions of -1 to 1V. The device was placed in a test gas chamber, 1V voltage was applied, and 1 to 100ppb concentration of NO2 was introduced, which enabled the sensing of trace NO2 gas.

[0064] like Figure 2 As shown, it is an optical microscope image of the Cu3HHTP2 / monolayer MoS2 device prepared in this embodiment. From the image, it can be seen that the Cu3HHTP2 / monolayer MoS2 covers the interdigital electrode area; Figure 3 As shown, this is a gas sensing performance diagram of the Cu3HHTP2 / single-layer MoS2 device prepared in this embodiment. It can be seen from the figure that the Cu3HHTP2 / single-layer MoS2 device can respond to NO2 in the ppb level concentration range.

[0065] Example 3

[0066] (1) transferring a few layers of hexagonal boron nitride grown by chemical vapor deposition onto a sapphire substrate, and preparing 10 nm thick Cr and 60 nm thick Au electrodes by vacuum evaporation to form a single-layer graphene device;

[0067] (2) Clean the surface of the few-layer hexagonal boron nitride by 50W plasma cleaning for 2 min in N2 atmosphere to remove defects;

[0068] (3) placing the defective few-layer hexagonal boron nitride device in an ethanol solution containing 1 mM copper acetate at -10°C for 20 minutes;

[0069] (4) The few-layer hexagonal boron nitride device was immersed in an ethanol solution containing 1 mM 2,3,6,7,10,11-hexahydroxytriphenylene for 20 min, and the immersion cycle was repeated three times to complete the growth of the second layer of the porous skeleton structure Cu3HHTP2;

[0070] (5) The sample surface was washed with ethanol solvent to remove the residual reactants, and then dried at 60°C to obtain a Cu3HHTP2 / few-layer hexagonal boron nitride device.

[0071] Tested by an electrochemical workstation, under the cyclic voltammetry test conditions of -1 to 1V, the device has a resistance greater than 10MΩ in dark light; when 1W of light of different wavelengths is passed through for testing, it can detect near-infrared and deep ultraviolet light, with a response speed as low as 100ms.

[0072] Example 4

[0073] (1) Transferring the single-layer graphene grown by chemical vapor deposition onto a polyimide substrate, and preparing 6 nm, 4 nm, and 8 nm thick Mo, Au, and Ag electrodes by vacuum evaporation to form a single-layer graphene device;

[0074] (2) Cleaning the surface of the monolayer graphene by 10W plasma cleaning for 1 min in an NH3 atmosphere to create defects;

[0075] (3) placing the defective single-layer graphene device in an ethanol solution containing 1 mM cobalt chloride at -5°C for 10 min;

[0076] (4) The single-layer graphene device was immersed in an ethanol solution containing 4 mM benzotriazole for 10 min, and the immersion cycle was repeated three times to complete the growth of the second layer of porous skeleton structure MOF;

[0077] (5) The sample surface was washed with ethanol solvent to remove residual reactants and dried at 60 °C to obtain a MOF / single-layer graphene flexible device.

[0078] Tested by an electrochemical workstation, the device resistance was less than 1kΩ under the cyclic voltammetry test conditions of -1 to 1V; the device was placed in a test gas chamber, a voltage of 1V was applied, and 1 to 10ppm concentration of toluene was introduced, and it was able to sense benzene gases under flexible bending conditions of 30°, 45°, and 60°.

[0079] Example 5

[0080] (1) transferring the multilayer polycrystalline MoS2 grown by chemical vapor deposition onto a polyethylene oxide substrate, and preparing 2 nm thick Cr and 20 nm thick Au electrodes by vacuum evaporation to form a multilayer polycrystalline MoS2 device;

[0081] (2) The surface of multilayer polycrystalline MoS2 was cleaned by 50W plasma cleaning for 2min in H2S atmosphere to remove defects;

[0082] (3) placing the defective multilayer polycrystalline MoS2 device in a methanol solution containing 1 mM zinc acetate and 1 mM cobalt acetate at -5°C for 20 min;

[0083] (4) The multilayer polycrystalline molybdenum disulfide device was immersed in a methanol solution containing 4 mM 2-methylimidazole for 20 min, and the immersion cycle was repeated three times to complete the growth of the second layer of porous framework structure ZIF;

[0084] (5) The sample surface was washed with methanol solvent to remove the residual reactants and freeze-dried at -50°C to obtain a ZIF / multilayer polycrystalline MoS2 device.

[0085] The device was tested on an electrochemical workstation and the resistance was about 10kΩ under the cyclic voltammetry test conditions of -1 to 1V. The device was used as an electrode, a voltage of 0.2V was applied, and 10μL of 100nM to 1mM concentration hydrogen peroxide solution was added to test the response current, which can realize the sensing of hydrogen peroxide at the nM level.

[0086] Example 6

[0087] (1) Transferring a single-layer polycrystalline MoS2 grown by chemical vapor deposition onto a Si / SiO2 substrate, and preparing a 5 nm thick Ti and a 50 nm thick Au electrode by vacuum evaporation to form a single-layer MoS2 device;

[0088] (2) Clean the surface of the monolayer polycrystalline MoS2 by 50W plasma cleaning for 2 min in N2 atmosphere to remove defects;

[0089] (3) placing the defective single-layer polycrystalline MoS2 device in a mixed solution of methanol and water containing 1 mM manganese acetate at -10°C for 20 minutes;

[0090] (4) The single-layer polycrystalline MoS2 device was immersed in a mixed solution of methanol and water containing 3 mM trimesic acid for 20 min, and the immersion cycle was repeated three times to complete the growth of the second layer of porous skeleton structure Mn(BTC);

[0091] (5) The sample surface was washed with a mixed solvent of methanol and water to remove the residual reactants, and then dried at 60°C to obtain a Mn(BTC) / single-layer polycrystalline MoS2 device.

[0092] Tested by an electrochemical workstation, under the cyclic voltammetry test conditions of -1 to 1V, the device resistance is about 100kΩ; using the device as a working electrode, introducing a counter electrode and a reference electrode, applying a voltage of 1V, and dropping 10μL of 0.5MH2SO4, it can successfully realize the anode hydrogen evolution reaction of the fuel cell, or in a 1M ZnSO4+MnSO4 electrolyte, it can realize the positive electrode zinc oxidation reaction of the aqueous zinc ion battery.

[0093] Comparative Example

[0094] (1) Transferring a monolayer of MoS2 grown by chemical vapor deposition onto a Si / SiO2 substrate, and preparing a 5 nm thick Ti and a 50 nm thick Au electrode by vacuum evaporation to form a monolayer MoS2 device;

[0095] (2) placing the monolayer MoS2 device in an ethanol solution containing 1 mM Cu(2+) acetate at -10°C for 20 min;

[0096] (3) The monolayer MoS2 device was immersed in an ethanol solution containing 1 mM 2,3,6,7,10,11-hexahydroxytriphenylene for 20 min, and the immersion cycle was repeated three times to complete the growth of the second layer of heterojunction Cu3HHTP2;

[0097] (4) The sample surface was washed with ethanol solvent to remove residual reactants and dried at 60°C to obtain a Cu3HHTP2 / single-layer MoS2 device.

[0098] Tested by an electrochemical workstation, under the cyclic voltammetry test conditions of -1 to 1V, the device resistance was about 10kΩ; but due to the lack of defects, Cu3HHTP2 was not successfully loaded on MoS2 to form a heterojunction. The device was placed in a test gas chamber, a voltage of 1V was applied, and 1 to 10ppm concentration of NO2 was introduced. The sensing performance of NO2 gas was poor.

[0099] like Figure 4 As shown, it is an optical microscope image of the Cu3HHTP2 / single-layer MoS2 device prepared in this comparative example. From the image, it can be seen that Cu3HHTP2 is almost invisible in the interdigital electrode area, indicating that the defective MoS2 failed to successfully form a heterostructure with Cu3HHTP2; Figure 5 As shown, this is the gas sensing performance diagram of the Cu3HHTP2 / single-layer molybdenum disulfide device prepared in this comparative example. It can be seen from the figure that the Cu3HHTP2 / single-layer molybdenum disulfide device hardly responds to ppm-level NO2, indicating that the device performance is poor.

[0100] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a defect-controlled two-dimensional material heterojunction device, characterized in that: The steps include: S1: Transfer the two-dimensional material to the substrate and prepare electrodes to form a two-dimensional material device; S2: Creating defects on the surface of 2D materials by plasma cleaning; S3: immersing the defective two-dimensional material device in a low-temperature metal ion solution; S4: immersing the immersed two-dimensional material device in the ligand solution again, and cyclically immersing the device to grow a second layer of porous skeleton structure material on the surface of the two-dimensional material to form a heterojunction; S5: cleaning and drying to obtain a defect-controlled two-dimensional material heterojunction device; in: The two-dimensional material is a single-layer graphene, a multi-layer graphene, a single-layer metal chalcogenide, a multi-layer metal chalcogenide, a single-layer hexagonal boron nitride or a multi-layer hexagonal boron nitride. The two-dimensional material is grown on a substrate by chemical vapor deposition and has a single-layer or few-layer structure. The low-temperature metal ion solution has a temperature of -40 to 5 °C, a solute of one or more of gold acetate, platinum acetate, silver acetate, palladium acetate, zinc acetate, cobalt acetate, copper acetate, manganese acetate, gold chlorate, platinum chlorate, silver chlorate, palladium chlorate, zinc chloride, cobalt chloride, copper chloride, manganese chloride, gold acetylacetonate, platinum acetylacetonate, silver acetylacetonate and palladium acetylacetonate, a solvent of one or more of ultrapure water, ethanol, methanol and isopropanol, and a solution concentration of 1 μM to 10 mM.

2. The method for preparing a defect-controlled two-dimensional material heterojunction device according to claim 1, characterized in that: In step S1, the substrate is Si / SiO2, polyester resin, polyethylene oxide, polyimide or sapphire, and the surface roughness of the substrate is less than 100 nm; the electrode is a metal electrode, and the metal is one or more of Al, Ni, Mo, Cu, Au, Ti, Cr, Nb, Ag, Pt and Pd, and the electrode thickness is less than 200 nm.

3. The method for preparing a defect-controlled two-dimensional material heterojunction device according to claim 1, characterized in that: In step S1, the electrode is prepared by vacuum evaporation or magnetron sputtering.

4. The method for preparing a defect-controlled two-dimensional material heterojunction device according to claim 1, characterized in that: In step S2, the plasma cleaning has a power of 10 to 1000 W, an atmosphere of one or more of argon, nitrogen, oxygen, ammonia and hydrogen sulfide, a gas flow rate of 10 to 1000 sccm, and a cleaning time of 1 to 10 min.

5. The method for preparing a defect-controlled two-dimensional material heterojunction device according to claim 1, characterized in that: In step S3, the soaking time is 1 to 60 min.

6. The method for preparing a defect-controlled two-dimensional material heterojunction device according to claim 1, characterized in that: In step S4, the ligand solution: the solute is one or more of imidazole derivatives, triphenylene derivatives, triazole derivatives and trimesic acid derivatives; the solvent is one or more of ultrapure water, ethanol, methanol and isopropanol; the concentration of the solution is 1 μM~10 mM; the immersion time is 1~60 min, and the number of repetitions is 2~10 times.

7. The method for preparing a defect-controlled two-dimensional material heterojunction device according to claim 1, characterized in that: In step S5, the cleaning solvent is one or more of ultrapure water, ethanol, methanol and isopropanol; the drying includes freeze drying and oven drying: when freeze drying is adopted, the freeze drying temperature is -10~-60°C, and when oven drying is adopted, the oven drying temperature is 50~100°C.

8. A defect-controlled two-dimensional material heterojunction device, characterized in that: The method is prepared by any one of claims 1 to 7.

9. Application of the defect-regulated two-dimensional material heterojunction device as claimed in claim 8 in electronic devices.

10. The use according to claim 9, characterized in that: The electronic devices include gas sensors, liquid sensors, photodetectors, flexible sensors, electrodes of lithium batteries, electrodes of fuel cells, electrodes of supercapacitors and light-emitting devices.