An agarose gel microsphere and a preparation method thereof
Patent Information
- Application Number
- CN202410184048.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-19
- Publication Date
- 2026-11-03
- Estimated Expiration
- 2044-02-19
AI Technical Summary
传统琼脂糖凝胶微球机械强度较低,难以同时满足高刚性、高流速和高载量的要求。
A method for preparing agarose gel microspheres involves using calcium carbonate-filled porous ceramic as a rigid core and treating it with an acidic solution to retain micron-sized flow pores, thereby improving mechanical strength and mass transfer performance.
This improves the mechanical strength and flowability of agarose gel microspheres, meeting the requirements of high flow rate and high loading, reducing column pressure, and enabling rapid separation of macromolecular solutes.
Smart Images

Figure BDA0004705200120000071
Abstract
Description
Technical Field
[0001] This invention belongs to the field of agarose gel media technology, specifically relating to an agarose gel microsphere and its preparation method. Background Technology
[0002] Chromatography is a technique that utilizes the differences in the physicochemical properties of different substances. It is one of the most effective methods for separating and purifying biomolecules such as monoclonal antibodies and nucleic acids. A chromatographic system consists of a stationary phase and a mobile phase. Due to the differences in the physicochemical properties of each component, their ability to interact with the two phases (adsorption, dissolution, binding, etc.) varies, resulting in different distributions (content ratios) between the two phases. Furthermore, as the mobile phase moves forward, the components continuously redistribute between the two phases. By collecting the eluent fractions, the individual components contained in the sample can be obtained, thus achieving the purpose of separating the components.
[0003] Porous gel microspheres are the most widely used chromatographic media for bioseparation in industry, and are mainly classified into natural polymers and synthetic polymers according to their source. Agarose is commonly used as a material for natural porous gel microspheres. The advantages of using agarose in the preparation of porous gel microspheres are its good water solubility, suitable gelation temperature, and high gel strength. However, with the rapid development of biotechnology, the demand for chromatographic media is constantly increasing, and the requirements are also constantly improving. Conventional natural porous gel microspheres are difficult to meet the requirements of high rigidity, high flow rate, and high loading capacity at the same time. Patent CN 114377629 A discloses a method for preparing chitosan-grafted agarose composite microspheres with large pore size and high loading capacity. It adopts a novel preparation and cross-linking method to graft chitosan onto agarose, which effectively improves the pore structure and cross-linking density inside the microspheres. Due to the modification of chitosan, it has higher mechanical strength and flow rate than traditional agarose microspheres. However, its process is relatively complex, the reaction conditions are demanding, and the resulting microspheres have uneven particle size, making it unsuitable for large-scale industrial chromatography. Summary of the Invention
[0004] The purpose of this invention is to provide an agarose gel microsphere and its preparation method to solve the problem of low mechanical strength of traditional agarose gel microspheres.
[0005] The objective of this invention can be achieved through the following technical solutions:
[0006] 1. A method for preparing agarose gel microspheres, characterized by comprising the following steps:
[0007] Step 1: Add the emulsifier to the organic solvent, heat and stir to obtain the organic phase; add agarose and calcium carbonate-filled porous ceramic to water, heat and stir to obtain the aqueous phase;
[0008] The second step is to add the aqueous phase to the organic phase and stir at 85°C for 15-20 minutes. Then, cool the temperature to 15-20°C and continue stirring for 30-40 minutes. Allow it to settle naturally to obtain microspheres. Add an epoxy crosslinking agent under alkaline conditions for crosslinking, then add sodium borohydride for reduction. After centrifugation, obtain the medium material.
[0009] The third step involves soaking the obtained medium material in an acidic solvent to remove calcium carbonate, followed by ultrasonic dispersion and centrifugation to obtain agarose gel microspheres.
[0010] As a preferred embodiment of the present invention, the organic solvent is at least one of cyclohexane and liquid paraffin.
[0011] As a preferred embodiment of the present invention, the emulsifier is at least one of Span 85, Span 80, and Span 60.
[0012] As a preferred embodiment of the present invention, the acidic solvent is hydrochloric acid with a concentration of 0.05-0.1 mol / L.
[0013] As a preferred embodiment of the present invention, the epoxy crosslinking agent is one of epichlorohydrin, ethylene glycol diglycidyl ether, butylene glycol diglycidyl ether, and hexanediol diglycidyl ether.
[0014] As a preferred embodiment of the present invention, calcium carbonate-filled porous ceramics are prepared by the following steps:
[0015] Porous ceramic micropowder is added to a saturated calcium hydroxide solution and soaked for 5-10 minutes. After filtration, it is dried under a carbon dioxide atmosphere. This soaking and drying process is repeated 5-10 times. Finally, the ceramic is pulverized and sieved to remove particles smaller than 10 μm and larger than 100 μm, yielding calcium carbonate-filled porous ceramics. Alternatively, the porous ceramic micropowder, after being soaked in a saturated calcium hydroxide aqueous solution, permeates into the pores of the ceramic micropowder. During the heating and drying process, it reacts with carbon dioxide in the gas to form solid calcium carbonate, filling the pores and resulting in calcium carbonate-filled porous ceramics.
[0016] As a preferred embodiment of the present invention, porous ceramic micro powder is prepared by the following steps:
[0017] Silicon carbide powder and alumina powder were mixed to obtain a mixed powder. Calcium carbonate and sodium carboxymethyl cellulose aqueous solution were added as binders. After ball milling and mixing, the mixture was molded, dried at 110℃ to constant weight, and sintered in air. After sintering, the mixture was cooled, ball milled, and sieved to obtain porous ceramic micro powder.
[0018] In a preferred embodiment of the present invention, the mass ratio of silicon carbide powder to alumina powder is 7:3; the amount of calcium carbonate added is 2% of the mass fraction of sodium carboxymethyl cellulose aqueous solution in the total mass of the mixed powder; the sintering temperature is 1300-1400℃; and the sintering time is 3-4 hours. The porous structure is mainly achieved through the pore-forming effect of the generated silicon carbide particles and CaCO3, and porous ceramic micropowder is obtained after ball milling.
[0019] As a preferred embodiment of the present invention, the porous ceramic micro powder has a particle size of 10-30 μm and a porosity of 20-40%.
[0020] An agarose gel microsphere was prepared by the above-described preparation method.
[0021] The beneficial effects of this invention are:
[0022] This invention provides a method for preparing agarose gel microspheres. The process is relatively simple. Calcium carbonate is used as a rigid additive to fill porous ceramic. After treatment with an acidic solution, micron-sized flow pores are retained, thus preparing agarose gel microspheres.
[0023] The agarose gel microspheres of this invention use calcium carbonate-filled porous ceramic as a rigid core, which improves the mechanical strength of the agarose gel microspheres and enables them to maintain a relatively stable state under high flow rate conditions. After the calcium carbonate-filled porous ceramic is introduced, it is treated with an acidic solution to retain the flow pores in the microspheres, forming a certain number of micron-sized flow pores, which enhances the mass transfer in the microspheres, increases the effective adsorption capacity, and enables the rapid separation of macromolecular (protein) solutes, while meeting the requirements of high rigidity, high flow rate, and high loading capacity.
[0024] In this invention, agarose gel microspheres prepared by filling porous ceramics with calcium carbonate can effectively reduce column pressure. This is because the porous ceramics filled with calcium carbonate not only play a certain role in creating pores, but also their rigid core can effectively improve the pore properties of the microspheres, maintain the stability of the micropores, improve the flowability of the medium, and thus improve the pressure resistance. Detailed Implementation
[0025] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0026] Example 1
[0027] This embodiment provides a calcium carbonate-filled porous ceramic prepared by the following steps:
[0028] Silicon carbide powder and alumina powder were mixed to obtain a mixed powder. Calcium carbonate and sodium carboxymethyl cellulose aqueous solution were added as binders. After ball milling and mixing, the mixture was molded, dried at 110℃ to constant weight, and sintered in air. After sintering, the powder was cooled, ball-milled, and sieved to obtain porous ceramic micropowder. The mass ratio of silicon carbide powder to alumina powder was 7:3; the amount of calcium carbonate added was 2% of the mass fraction of sodium carboxymethyl cellulose aqueous solution in the total mass of the mixed powder; the sintering temperature was 1300℃; the sintering time was 3 hours; the particle size of the porous ceramic micropowder was 10-30 μm; and the porosity of the porous ceramic micropowder was 20-30%.
[0029] Porous ceramic micropowder was added to a saturated calcium hydroxide solution and soaked for 10 minutes. After filtration, the mixture was dried under a carbon dioxide atmosphere. This soaking and drying process was repeated five times. Finally, the ceramic was pulverized and sieved to remove particles smaller than 10 μm and larger than 100 μm, yielding calcium carbonate-filled porous ceramics. Alternatively, the porous ceramic micropowder, after being soaked in a saturated calcium hydroxide aqueous solution, permeates into the pores of the ceramic micropowder. During the heating and drying process, it reacts with carbon dioxide in the gas to form solid calcium carbonate, which fills the pores, resulting in calcium carbonate-filled porous ceramics.
[0030] Example 2
[0031] This embodiment provides a calcium carbonate-filled porous ceramic prepared by the following steps:
[0032] Silicon carbide powder and alumina powder were mixed to obtain a mixed powder. Calcium carbonate and sodium carboxymethyl cellulose aqueous solution were added as binders. After ball milling and mixing, the mixture was molded, dried at 110℃ to constant weight, and sintered in air. After sintering, the powder was cooled, ball-milled, and sieved to obtain porous ceramic micropowder. The mass ratio of silicon carbide powder to alumina powder was 7:3; the amount of calcium carbonate added was 2% of the total mass of the mixed powder and the mass fraction of sodium carboxymethyl cellulose aqueous solution; the sintering temperature was 1400℃, and the sintering time was 4 hours; the particle size of the porous ceramic micropowder was 10-30 μm; and the porosity of the porous ceramic micropowder was 30-40%.
[0033] Porous ceramic micropowder was added to a saturated calcium hydroxide solution and soaked for 5 minutes. After filtration, the mixture was dried under a carbon dioxide atmosphere. This soaking and drying process was repeated 10 times. Afterward, the ceramic was pulverized and sieved to remove particles smaller than 10 μm and larger than 100 μm, yielding calcium carbonate-filled porous ceramic. Alternatively, the porous ceramic micropowder, after being soaked in a saturated calcium hydroxide aqueous solution, permeates into the pores of the ceramic micropowder. During the heating and drying process, it reacts with carbon dioxide in the gas to form solid calcium carbonate, filling the pores and resulting in calcium carbonate-filled porous ceramic.
[0034] Example 3
[0035] This embodiment provides a method for preparing agarose gel microspheres, including the following steps:
[0036] Step 1: Add Span 80 to liquid paraffin, heat and stir to obtain the organic phase; add agarose and calcium carbonate-filled porous ceramic prepared according to the method in Example 1 to water, heat and stir to obtain the aqueous phase;
[0037] Step 2: While stirring at 2000 rpm, the aqueous phase was added to the organic phase. The mixture was stirred at 85℃ for 15 min, then cooled to 15℃ and stirred for another 30 min. After natural sedimentation, microspheres were obtained. These microspheres were washed repeatedly with acetone and distilled water. 5 g of the washed microspheres were added to 100 mL of water to adjust the system to alkaline (pH 11). 5 mL of epichlorohydrin was added, and the mixture was stirred for 5 h. After the reaction was completed, 0.5 g of sodium borohydride was added, and the mixture was stirred for another 6 h. The media material was obtained by centrifugation.
[0038] The third step involves soaking the obtained medium material in 0.06 mol / L hydrochloric acid for 30 minutes to remove calcium carbonate, followed by ultrasonic dispersion and centrifugation to obtain agarose gel microspheres.
[0039] Example 4
[0040] This embodiment provides a method for preparing agarose gel microspheres, including the following steps:
[0041] Step 1: Add Span 80 to liquid paraffin, heat and stir to obtain the organic phase; add agarose and calcium carbonate-filled porous ceramic prepared according to the method in Example 2 to water, heat and stir to obtain the aqueous phase;
[0042] Step 2: While stirring at 3000 rpm, the aqueous phase was added to the organic phase. The mixture was stirred at 85℃ for 20 min, then cooled to 20℃ and stirred for another 40 min. After natural sedimentation, microspheres were obtained. These microspheres were washed repeatedly with acetone and distilled water. 5 g of the washed microspheres were added to 100 mL of water to adjust the system to alkaline (pH 12). 5 mL of epichlorohydrin was added, and the mixture was stirred for 5 h. After the reaction was completed, 0.5 g of sodium borohydride was added, and the mixture was stirred for another 5 h. The media material was obtained by centrifugation.
[0043] The third step involves soaking the obtained medium material in 0.1 mol / L hydrochloric acid for 20 minutes to remove calcium carbonate, followed by ultrasonic dispersion and centrifugation to obtain agarose gel microspheres.
[0044] Example 5
[0045] Compared with Example 4, this embodiment replaces liquid paraffin with cyclohexane; the emulsifier is Span 85.
[0046] Example 6
[0047] Compared with Example 4, the epoxy crosslinking agent in this embodiment is ethylene glycol diglycidyl ether.
[0048] Example 7
[0049] Compared with Example 4, the epoxy crosslinking agent in this embodiment is hexanediol diglycidyl ether.
[0050] Comparative Example 1
[0051] Compared to Example 4, this comparative example replaces the calcium carbonate-filled porous ceramic with the porous ceramic powder from Example 1, without the hydrochloric acid soaking treatment. All other raw materials and preparation processes remain the same as in Example 4.
[0052] Comparative Example 2
[0053] Compared with Example 4, this comparative example replaces calcium carbonate-filled porous ceramic with calcium carbonate, while the other raw materials and preparation process remain the same as in Example 4.
[0054] Performance tests were performed on the samples prepared in Examples 3-7 and Comparative Examples 1-2:
[0055] Column pressure tolerance: A column (1 cm inner diameter, 4.46 cm height) was packed with 3.5 mL of medium and connected to an AKTAPurifier chromatography system. The mobile phase was 0.1 mol / L NaCl. The column pressure (MPa) at different flow rates was measured. The results are shown in Table 1.
[0056] Table 1
[0057]
[0058] As shown in Table 1, the agarose gel microspheres prepared by calcium carbonate-filled porous ceramics in this invention can effectively reduce column pressure. This is because the calcium carbonate-filled porous ceramics not only play a certain role in creating pores, but their rigid core can also effectively improve the pore properties of the microspheres, maintain the stability of the micropores, improve the flowability of the medium, and thus improve the pressure resistance. Compared with the samples prepared in the examples, the samples prepared in Comparative Example 1 have fewer or no internal micropores, resulting in relatively higher flowability. However, due to their rigid content, they can still maintain relatively stable column pressure under high flow rate conditions.
[0059] The samples prepared in Example 4 and Comparative Examples 1-2 were tested. The samples were modified, and then a protein adsorption experiment was performed.
[0060] The sample was added to a 1 mol / L sodium hydroxide solution, followed by 1 mol / L DEAE-Cl (diethylaminochloroethane hydrochloride). The mixture was stirred at 60°C for 90-100 min. After the reaction, the sample was filtered, washed with 50% (v / v) ethanol aqueous solution, and dried to obtain the test sample. The static and dynamic adsorption capacities of bovine serum albumin (BSA) were measured (unit: mg BSA / mL wet microspheres). The dynamic adsorption capacity was determined at a flow rate of 800 cm / h. Five groups were tested under the same conditions, and the average value was calculated. The test results are shown below:
[0061] Table 2
[0062] Test sample Static adsorption capacity Dynamic adsorption capacity Example 4 284.0 64.0 Comparative Example 1 195.0 38.0 Comparative Example 2 131.0 15.0
[0063] The test results show that the medium material prepared by this invention has better adsorption capacity and stability.
[0064] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0065] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing agarose gel microspheres, characterized in that, Includes the following steps: Step 1: Add the emulsifier to the organic solvent, heat and stir to obtain the organic phase; add agarose and calcium carbonate-filled porous ceramic to water, heat and stir to obtain the aqueous phase; The second step is to add the aqueous phase to the organic phase and stir at 85°C for 15-20 minutes. Then, cool the temperature to 15-20°C and continue stirring for 30-40 minutes. Allow it to settle naturally to obtain microspheres. Add an epoxy crosslinking agent under alkaline conditions for crosslinking, then add sodium borohydride for reduction. After centrifugation, obtain the medium material. The third step involves soaking the obtained medium material in an acidic solvent to remove calcium carbonate, followed by ultrasonic dispersion and centrifugation to obtain agarose gel microspheres.
2. The method for preparing agarose gel microspheres according to claim 1, characterized in that, The organic solvent is at least one of cyclohexane and liquid paraffin.
3. The method for preparing agarose gel microspheres according to claim 1, characterized in that, The emulsifier is at least one of Span 85, Span 80, and Span 60.
4. The method for preparing agarose gel microspheres according to claim 1, characterized in that, The acidic solvent is 0.05-0.1 mol / L hydrochloric acid.
5. The method for preparing agarose gel microspheres according to claim 1, characterized in that, The epoxy crosslinking agent is one of epichlorohydrin, ethylene glycol diglycidyl ether, butylene glycol diglycidyl ether, and hexanediol diglycidyl ether.
6. The method for preparing agarose gel microspheres according to claim 1, characterized in that, Calcium carbonate-filled porous ceramics are prepared through the following steps: Porous ceramic micropowder is added to a saturated calcium hydroxide solution and soaked for 5-10 minutes. After filtration and separation, the powder is dried under a carbon dioxide atmosphere. The soaking and drying process is repeated 5-10 times. After the process is completed, the powder is crushed and sieved to remove the portions smaller than 10 μm and larger than 100 μm, thus obtaining calcium carbonate-filled porous ceramic.
7. The method for preparing agarose gel microspheres according to claim 6, characterized in that, Porous ceramic micro powder is prepared through the following steps: Silicon carbide powder and alumina powder were mixed to obtain a mixed powder. Calcium carbonate and sodium carboxymethyl cellulose aqueous solution were added as binders. After ball milling and mixing, the mixture was molded, dried at 110℃ to constant weight, and sintered in air. After sintering, the mixture was cooled, ball milled, and sieved to obtain porous ceramic micro powder.
8. The method for preparing agarose gel microspheres according to claim 7, characterized in that, The mass ratio of silicon carbide powder to alumina powder is 7:3; the amount of calcium carbonate added is 2% of the total mass of the mixed powder and the mass fraction of sodium carboxymethyl cellulose aqueous solution; the sintering temperature is 1300-1400℃ and the sintering time is 3-4h.
9. The method for preparing agarose gel microspheres according to claim 6, characterized in that, The particle size of the porous ceramic powder is 10-30 μm; the porosity of the porous ceramic powder is 20-40%.
10. An agarose gel microsphere, characterized in that, It is prepared by the preparation method according to any one of claims 1-9.
Citation Information
Patent Citations
Preparation method of large-aperture high-loading chitosan grafted agarose composite microspheres
CN114377629A
Macroporous agarose microspheres and preparation method thereof
CN103055773A
Prepn. method of macroporous Ago-Gel medium
CN1868578A