Metallic glass-carbide composite material and preparation method thereof

By introducing high-entropy carbide powder into a metallic glass matrix, a metallic glass-carbide composite material is formed, which solves the brittleness problem of bulk metallic glass, achieves a combination of high strength and high plasticity, and enhances the mechanical properties of the material.

CN118326197BActive Publication Date: 2024-11-19CHONGQING NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410525193.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-11-19
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

Large metallic glasses lack the ability to undergo plastic deformation at room temperature, leading to catastrophic brittle fracture after the yield point, which limits their application as structural and engineering materials.

Method used

By mixing high-entropy carbide powder TiZrHfNbTaC5 with a metallic glass matrix Zr53Cu30Ni9Al8 and rapidly cooling it, a metallic glass-carbide composite material is formed. The carbide powder acts as a second phase, uniformly dispersed in the matrix, hindering shear band expansion and promoting the derivation of multiple shear bands.

Benefits of technology

It significantly improves the plastic strain and fracture strength of the material, enhances the overall mechanical properties of the material, with a compressive strain of about 8%, and a significant improvement in fracture strength and hardness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118326197B_ABST
    Figure CN118326197B_ABST
Patent Text Reader

Abstract

The present invention provides a metallic glass-carbide composite material and a preparation method thereof. The composite material has a general formula I: (Zr 53 Cu 30 Ni9Al8) 100‑x (TiZrHfNbTaC5) x Formula I; x is atomic percentage, 0<x≤10. The present invention retains the excellent fracture strength and hardness of the metallic glass matrix, and adds high entropy carbide powder as the second phase, so that the plasticity of the material is significantly improved. The obtained composite material has a compression strain of about 8%, which is much better than the metallic glass matrix, and further improves the fracture strength and hardness of the material, and enhances the overall mechanical properties of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and in particular relates to a metallic glass-carbide composite material and a preparation method thereof. Background Art

[0002] Compared with traditional crystalline alloys, bulk metallic glasses have attracted extensive attention due to their high strength, elastic limit, hardness and excellent corrosion resistance. However, the lack of room temperature plastic deformation ability of bulk metallic glasses has seriously hindered their application as structural and engineering materials. The plastic strain of bulk metallic glasses is usually concentrated in one or several major shear bands due to their unique amorphous microstructure, so catastrophic brittle fracture occurs after the yield point occurs. Therefore, improving the ductility of bulk metallic glasses is of great significance to improving their application performance. Summary of the invention

[0003] In view of this, an object of the present invention is to provide a metallic glass-carbide composite material and a preparation method thereof, wherein the composite material has excellent plasticity.

[0004] The present invention provides a metallic glass-carbide composite material having a general formula I:

[0005] (Zr 53 Cu 30 Ni 9 Al 8 ) 100-x (TiZrHfNbTaC 5 ) x Formula I;

[0006] x is atomic percentage, 0<x≤10.

[0007] Preferably, 2≤x≤10.

[0008] The present invention provides a method for preparing the metallic glass-carbide composite material described in the above technical solution, comprising the following steps:

[0009] The molten metallic glass matrix Zr 53 Cu 30 Ni 9 Al 8 and carbide powder TiZrHfNbTaC 5 The mixture is mixed and cooled to obtain a metallic glass-carbide composite material.

[0010] Preferably, the cooling rate is greater than or equal to 120K / s.

[0011] Preferably, the molten metallic glass matrix Zr 53 Cu 30 Ni9 Al 8 and carbide powder TiZrHfNbTaC 5 Mix includes:

[0012] The metallic glass matrix Zr was prepared by suction casting. 53 Cu 30 Ni 9 Al 8 The molten liquid is sucked into the carbide powder TiZrHfNbTaC 5 In the copper mold;

[0013] Or carbide powder TiZrHfNbTaC 5 Adhesion to metallic glass Zr 53 Cu 30 Ni 9 Al 8 on the molten liquid.

[0014] Preferably, the molten metallic glass matrix Zr 53 Cu 30 Ni 9 Al 8 Prepared according to the following method:

[0015] The metal element constituting the metallic glass is placed in an argon environment adsorbed by sponge titanium to be melted to obtain a master alloy ingot of the metallic glass, and the melting temperature is 2000°C to 2100°C.

[0016] Preferably, the carbide powder TiZrHfNbTaC 5 The particle size is 5 to 50 μm.

[0017] Preferably, the purity of the metallic glass matrix and the carbide powder is not less than 99.99%.

[0018] The present invention provides a metallic glass-carbide composite material having a general formula I: (Zr 53 Cu 30 Ni 9 Al 8 ) 100-x (TiZrHfNbTaC 5 ) x Formula I; x is atomic percentage, 0<x≤10. The present invention retains the excellent fracture strength and hardness of the metallic glass matrix, and adds high entropy carbide powder as the second phase, so that the plasticity of the material is significantly improved. The obtained composite material has a compression strain of about 8%, which is much better than the metallic glass matrix, and further improves the fracture strength and hardness of the material, and enhances the overall mechanical properties of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The (Zr) prepared in Example 2 of the present invention 53 Cu 30 Ni 9 Al 8 ) 95 (TiZrHfNbTaC 5 ) 5 Composite materials and TiZrHfNbTaC 5 X-ray diffraction pattern of the sample;

[0020] Figure 2 The (Zr) prepared in Example 2 of the present invention 53 Cu 30 Ni 9 Al 8 ) 95 (TiZrHfNbTaC 5 ) 5 Composite materials and Zr 53 Cu 30 Ni 9 Al 8 DSC curve of amorphous alloy at a heating rate of 20K / s;

[0021] Figure 3 The (Zr) prepared in Example 2 of the present invention 53 Cu 30 Ni 9 Al 8 ) 95 (TiZrHfNbTaC 5 ) 5 Composite material Zr 53 Cu 30 Ni 9 Al 8 Stress-strain images of amorphous alloys and Zr 53 Cu 30 Ni 9 Al 8 Refer to the figure for metallic glass;

[0022] Figure 4 (Zr prepared in Example 2 of the present invention 53 Cu 30 Ni 9 Al 8 ) 95 (TiZrHfNbTaC 5 ) 5 Surface morphology of composite materials;

[0023] Figure 5 (Zr prepared in Example 2 of the present invention 53 Cu 30 Ni9 Al 8 ) 95 (TiZrHfNbTaC 5 ) 5 Fracture side morphology of the composite material;

[0024] Figure 6 (Zr prepared in Example 2 of the present invention 53 Cu 30 Ni 9 Al 8 ) 95 (TiZrHfNbTaC 5 ) 5 Fracture surface morphology of the composite material. DETAILED DESCRIPTION

[0025] The present invention provides a metallic glass-carbide composite material having a general formula I:

[0026] (Zr 53 Cu 30 Ni 9 Al 8 ) 100-x (TiZrHfNbTaC 5 ) x Formula I;

[0027] x is the atomic percentage, 0 <x≤10。

[0028] The composite material of the present invention is made of metallic glass Zr 53 Cu 30 Ni 9 Al 8 As the matrix, high entropy carbide TiZrHfNbTaC is deposited on the surface and inside of the matrix. 5 The composite material is formed by melting high entropy carbide powder into a molten liquid of metallic glass and then rapidly cooling it.

[0029] The x is the atomic percentage, at%, which means the carbide accounts for Zr 53 Cu 30 Ni 9 Al 8 The atomic percentage of x is a natural number; preferably, 2≤x≤10; specifically, x=2, x=3, x=4, x=5, x=6, x=7, x=8, x=9 or x=10.

[0030] The present invention uses Zr 53 Cu 30 Ni 9 Al 8Metallic glass is used as the matrix, high entropy carbides are deposited on the surface and inside of the matrix, and carbide powder TiZrHfNbTaC is introduced 5 It can make the composite material have excellent plasticity, and can further improve the strength and hardness of the matrix and enhance the overall mechanical properties of the material.

[0031] The present invention provides a method for preparing the metallic glass-carbide composite material described in the above technical solution, comprising the following steps:

[0032] The molten metallic glass matrix Zr 53 Cu 30 Ni 9 Al 8 and carbide powder TiZrHfNbTaC 5 The mixture is mixed and cooled to obtain a metallic glass-carbide composite material.

[0033] The metallic glass-high entropy carbide composite material prepared by the method provided by the present invention overcomes the disadvantage of room temperature brittleness of metallic glass and has excellent mechanical properties of high strength and high plasticity.

[0034] In the present invention, the molten metallic glass matrix Zr 53 Cu 30 Ni 9 Al 8 Prepared according to the following method:

[0035] The metal element constituting the metallic glass is placed in an argon environment adsorbed by sponge titanium to be melted to obtain a master alloy ingot of the metallic glass, and the melting temperature is 2000°C to 2100°C.

[0036] The purity of the metal element constituting the metallic glass is not less than 99.99%.

[0037] The molten metallic glass matrix Zr 53 Cu 30 Ni 9 Al 8 and carbide powder TiZrHfNbTaC 5 Mix includes:

[0038] The metallic glass matrix Zr was prepared by suction casting. 53 Cu 30 Ni 9 Al 8 The molten liquid is sucked into the carbide powder TiZrHfNbTaC 5 In the copper mold;

[0039] Or carbide powder TiZrHfNbTaC 5 Adhesion to metallic glass Zr 53Cu 30 Ni 9 Al 8 on the molten liquid.

[0040] The present invention absorbs the molten liquid of the metallic glass matrix into the carbide powder TiZrHfNbTaC by pressure difference. 5 The cooling rate in the present invention is greater than or equal to 120K / s.

[0041] The TiZrHfNbTaC 5 Preferably, it is prepared by the following method:

[0042] Mixing metal powders of Ti, Zr, Hf, Nb, and Ta and powder of a single substance of C according to a set molar ratio to obtain a mixture;

[0043] The powder mixture is placed in a hexagonal large cavity press and maintained at 2200°C to 2400°C and 4.5 to 5.5 GPa pressure for 10 to 20 minutes to obtain high entropy carbide TiZrHfNbTaC5.

[0044] Specifically, according to Zr 53 Cu 30 Ni 9 Al 8 The nominal composition is a metal element zirconium, copper, nickel, and aluminum with a purity of not less than 99.9%. The metal element zirconium, copper, nickel, and aluminum are placed in an argon environment with titanium inhalation, and the arc is repeatedly melted for more than 5 times to make the elements evenly distributed. The melting temperature is controlled at 2000℃~2100℃ to obtain Zr 53 Cu 30 Ni 9 Al 8 Master alloy ingot;

[0045] The carbide powder is placed in the spherical cavity of the copper mold, a screw is screwed on the bottom of the copper mold to prevent the powder from leaking out, and the copper mold is placed in a non-consumable vacuum arc furnace;

[0046] The prepared master alloy ingot is placed on the top of the copper mold. After the master alloy ingot is melted into molten liquid again, the molten liquid and high-entropy carbide powder are quickly sucked into the copper mold through the pressure difference between the furnace cavity and the copper mold, so that the high-entropy carbide is dispersed in the master alloy, and then rapidly cooled. The rapid cooling rate is not less than 120K / s, and a metallic glass-carbide composite material with excellent mechanical properties can be obtained.

[0047] The purity of the carbide powder used in the present invention is not less than 99.99%. The carbide powder TiZrHfNbTaC 5The particle size is 5 to 50 μm. The carbide powder is a high entropy carbide material with an entropy value of S>1.61R. The carbide as a second phase, when the composite material is subjected to an external load, the second phase particles are uniformly dispersed in the metallic glass matrix, which hinders the rapid expansion of the shear band and promotes the derivation of multiple shear bands, thereby greatly reducing the disadvantage that the metallic glass is prone to catastrophic fracture under high pressure.

[0048] The preparation method provided by the invention is simple and easy to operate, can involve components by itself, and has excellent mechanical properties.

[0049] Mechanical testing was performed using a microcomputer-controlled electronic universal testing machine RG / M-4300.

[0050] In order to further illustrate the present invention, a metallic glass-carbide composite material and a preparation method thereof provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0051] Example 1

[0052] The composition of the bulk metallic glass-high entropy carbide composite material prepared in this embodiment is expressed by the chemical formula: (Zr 53 Cu 30 Ni 9 Al 8 ) 98 (TiZrHfNbTaC 5 ) 2 ; Its preparation method comprises the following steps:

[0053] a. Take metal elements zirconium, copper, nickel and aluminum with a purity of not less than 99.9% and place them in an argon environment adsorbed by titanium, mix and smelt them 5 times, each time for 30 seconds, and control the smelting temperature at 2000℃~2100℃ to obtain Zr 53 Cu 30 Ni 9 Al 8 Master alloy ingot;

[0054] b. Physically mix metal powders of Ti, Zr, Hf, Nb, Ta and powder of a single substance of C according to a set molar ratio; place the powder mixture in a six-sided top large cavity press, and keep it in an environment of 2300°C and 5GPa pressure for 15 minutes to obtain high entropy carbide TiZrHfNbTaC5 with a particle size of 5 to 50 μm;

[0055] A high entropy carbide powder with a particle size of 5 to 50 μm is placed in a spherical cavity of a copper mold, a screw is screwed on the bottom of the copper mold to prevent the powder from leaking out, and the copper mold is placed in a non-consumable vacuum arc furnace;

[0056] c. Placing the master alloy ingot obtained in step a on the top of the copper mold, and melting the master alloy ingot into molten liquid again, rapidly sucking the molten liquid together with the high entropy carbide powder into the copper mold through the pressure difference between the furnace cavity and the inside of the copper mold, so that the high entropy carbide is dispersed in the master alloy, and then rapidly cooling, with the rapid cooling rate not less than 120K / s, to obtain a metallic glass-high entropy carbide composite material with excellent mechanical properties.

[0057] The columnar composite material with a diameter of 3 mm and a length of 6 mm prepared in this embodiment is 53 Cu 30 Ni 9 Al 8 The compression test data of the matrix alloy sample at a compression rate of 0.036 mm / min are shown in Table 1:

[0058] Table 1

[0059]

[0060] Example 2

[0061] The composition of the bulk metallic glass-high entropy carbide composite material prepared in this embodiment is expressed by the chemical formula: (Zr 53 Cu 30 Ni 9 Al 8 ) 95 (TiZrHfNbTaC 5 ) 5 ; Its preparation method comprises the following steps:

[0062] a. Take metal elements zirconium, copper, nickel and aluminum with a purity of not less than 99.9% and place them in an argon environment adsorbed by titanium, mix and smelt them 5 times, each time for 30 seconds, and control the smelting temperature at 2000℃~2100℃ to obtain Zr 53 Cu 30 Ni 9 Al 8 Master alloy ingot;

[0063] b. Physically mix metal powders of Ti, Zr, Hf, Nb, Ta and powder of a single substance of C according to a set molar ratio; place the powder mixture in a six-sided top large cavity press, and keep it in an environment of 2300°C and 5GPa pressure for 15 minutes to obtain high entropy carbide TiZrHfNbTaC5 with a particle size of 5 to 50 μm;

[0064] High entropy carbide powder with a particle size of 5 to 50 is placed in a spherical cavity of a copper mold, a screw is screwed on the bottom of the copper mold to prevent the powder from leaking out, and the copper mold is placed in a non-consumable vacuum arc furnace;

[0065] c. Placing the master alloy ingot obtained in step a on the top of the copper mold, and melting the master alloy ingot into molten liquid again, rapidly sucking the molten liquid together with the high entropy carbide powder into the copper mold through the pressure difference between the furnace cavity and the inside of the copper mold, so that the high entropy carbide is dispersed in the master alloy, and then rapidly cooling, with the rapid cooling rate not less than 120K / s, to obtain a metallic glass-high entropy carbide composite material with excellent mechanical properties.

[0066] The columnar (Zr) with a diameter of 3 mm and a length of 6 mm prepared in this embodiment 53 Cu 30 Ni 9 Al 8 ) 95 (TiZrHfNbTaC 5 ) 5 Composite materials and Zr 53 Cu 30 Ni 9 Al 8 The compression test data of the matrix alloy sample at a compression rate of 0.036 mm / min are shown in Table 2:

[0067] Table 2

[0068]

[0069] Example 3

[0070] The composition of the bulk metallic glass-high entropy carbide composite material prepared in this embodiment is expressed by the chemical formula: (Zr 53 Cu 30 Ni 9 Al 8 ) 90 (TiZrHfNbTaC 5 ) 10 ; Its preparation method comprises the following steps:

[0071] a. Take metal elements zirconium, copper, nickel and aluminum with a purity of not less than 99.9% and place them in an argon environment adsorbed by titanium, mix and smelt them 5 times, each time for 30 seconds, and control the smelting temperature at 2000℃~2100℃ to obtain Zr 53 Cu 30 Ni 9 Al 8 Master alloy ingot;

[0072] b. Physically mix metal powders of Ti, Zr, Hf, Nb, Ta and powder of a single substance of C according to a set molar ratio; place the powder mixture in a six-sided top large cavity press, and keep it in an environment of 2300°C and 5GPa pressure for 15 minutes to obtain high entropy carbide TiZrHfNbTaC5 with a particle size of 5 to 50 μm;

[0073] A high entropy carbide powder with a particle size of 5 to 50 μm is placed in a spherical cavity of a copper mold, a screw is screwed on the bottom of the copper mold to prevent the powder from leaking out, and the copper mold is placed in a non-consumable vacuum arc furnace;

[0074] c. Placing the master alloy ingot obtained in step a on the top of the copper mold, and melting the master alloy ingot into molten liquid again, rapidly sucking the molten liquid together with the high entropy carbide powder into the copper mold through the pressure difference between the furnace cavity and the inside of the copper mold, so that the high entropy carbide is dispersed in the master alloy, and then rapidly cooling, with the rapid cooling rate not less than 120K / s, to obtain a metallic glass-high entropy carbide composite material with excellent mechanical properties.

[0075] The columnar (Zr) with a diameter of 3 mm and a length of 6 mm prepared in this embodiment 53 Cu 30 Ni 9 Al 8 ) 90 (TiZrHfNbTaC 5 ) 10 Composite materials and Zr 53 Cu 30 Ni 9 Al 8 The compression test data of the matrix alloy sample at a compression rate of 0.036 mm / min are shown in Table 3:

[0076] Table 3

[0077]

[0078] From the above examples, it can be seen that the present invention provides a metallic glass-carbide composite material having the general formula I: (Zr 53 Cu 30 Ni 9 Al 8 ) 100-x (TiZrHfNbTaC 5 ) x Formula I; x is atomic percentage, 0<x≤10. The present invention retains the excellent fracture strength and hardness of the metallic glass matrix while adding high entropy carbide powder as the second phase, so that the plasticity of the material is significantly improved. The obtained composite material has a compression strain of about 8%, which is far superior to the metallic glass matrix. It also further improves the fracture strength and hardness of the material and enhances the overall mechanical properties of the material. The test results show that when the composite material is compressed at a compression rate of 0.036mm / min, the fracture strength is 1.96~2.02GPa, the elastic strain is 2.53~2.83%, and the plastic strain is 2.40~5.40%.

[0079] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A metallic glass-carbide composite material having the general formula I: (Zr 53 Cu 30 Ni9Al8) 100-x (TiZrHfNbTaC5) x Formula I; x is atomic percentage, 0<x≤10.

2. The metallic glass-carbide composite material according to claim 1, characterized in that: 2≤x≤10。 3. A method for preparing the metallic glass-carbide composite material according to any one of claims 1 to 2, comprising the following steps: The molten metallic glass matrix Zr 53 Cu 30 Ni9Al8 and carbide powder TiZrHfNbTaC5 are mixed and cooled to obtain a metallic glass-carbide composite material.

4. The preparation method according to claim 3, characterized in that: The cooling rate is greater than or equal to 120K / s.

5. The preparation method according to claim 3, characterized in that: The molten metallic glass matrix Zr 53 Cu 30 Ni9Al8 and carbide powder TiZrHfNbTaC5 mixed including: The metallic glass matrix Zr was prepared by suction casting. 53 Cu 30 The molten liquid of Ni9Al8 is sucked into a copper mold filled with carbide powder TiZrHfNbTaC5; Or adhere carbide powder TiZrHfNbTaC5 to metallic glass Zr 53 Cu 30 On the molten liquid of Ni9Al8.

6. The preparation method according to claim 3, characterized in that: The molten metallic glass matrix Zr 53 Cu 30 Ni9Al8 is prepared according to the following method: The metal element constituting the metallic glass is placed in an argon environment adsorbed by sponge titanium to be melted to obtain a master alloy ingot of the metallic glass, and the melting temperature is 2000°C to 2100°C.

7. The preparation method according to claim 3, characterized in that: The particle size of the carbide powder TiZrHfNbTaC5 is 5 to 50 μm.

8. The preparation method according to claim 3, characterized in that: The purity of the metallic glass matrix and the carbide powder is not less than 99.99%.