A vapor deposition method for increasing the voltage of SCR products

By using pulse power supply and reactive gas control technology in SCR products, the plasma excitation degree and film deposition efficiency are improved, and the problem of poor voltage performance in existing vapor deposition methods is solved, and high-quality thin film deposition and voltage performance are achieved promote.

CN118326379BActive Publication Date: 2024-11-19JIANGSU SEMICON CHAMPION MICROELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410449945.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-15
Publication Date
2024-11-19
Estimated Expiration
2044-04-15

AI Technical Summary

Technical Problem

The existing vapor deposition methods have problems such as low plasma excitation, poor film deposition quality, and improper control of reaction gases in SCR products, resulting in poor voltage performance.

Method used

Power is powered by pulse power supply, the flow rate and pressure of the reaction gas, the pulse duration of the reaction gas is controlled, and the carrier pretreatment and post-deposition treatment steps are combined to improve the plasma excitation degree and film deposition efficiency.

Benefits of technology

It improves the voltage performance of SCR products, achieves uniform, fast and high-quality deposition of films, enhances the stability and uniformity of plasma, and improves the voltage and deposition rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118326379B_ABST
    Figure CN118326379B_ABST
Patent Text Reader

Abstract

The present invention discloses a vapor deposition method for increasing the voltage of SCR products, which relates to the technical field of SCR product processing, and includes the following steps: S1, carrier pretreatment; S2, catalyst precursor gas preparation; S3, conductive layer vapor deposition; S4, deposition post-treatment. The present invention enhances the excitation degree of plasma. Radio frequency power is the main energy source for exciting plasma. Increasing radio frequency power can increase the density and temperature of plasma, increase the excitation degree of voltage-enhanced plasma, improve the efficiency of chemical reactions and the rate of thin film deposition, and achieve effective chemical reactions without significantly increasing the temperature of the substrate electrode. A more uniform electric field distribution is generated in the reaction chamber to improve the uniformity of plasma, achieve uniform, rapid and high-quality deposition of thin films, and improve the voltage performance of SCR products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of SCR product processing, and in particular to a vapor deposition method for increasing the voltage of an SCR product. Background Art

[0002] There are several types of thyristor rectifiers: unidirectional, bidirectional, switchable and light-controlled. They have the advantages of small size, light weight, high efficiency, long life and easy control. They are widely used in various automatic control and high-power power conversion occasions such as controlled rectification, voltage regulation, inversion and contactless switching. The anode and cathode of the thyristor rectifier are its core parts, responsible for the input and output of current. Depositing thin films or coatings on these surfaces can improve current distribution, enhance conductivity and enhance the corrosion resistance of the material.

[0003] The defects of the vapor deposition method in the prior art are:

[0004] 1. Patent document JP2004289035A discloses a chemical vapor deposition method and a chemical vapor deposition device. The chemical vapor deposition method cannot adjust the radio frequency power, the plasma chemical reaction efficiency of the raw material gas is low, and the film deposition quality is poor.

[0005] 2. Patent document CN107012448B discloses a radio frequency plasma enhanced chemical vapor deposition method and device. The vapor deposition method uses a DC power supply to control the plasma. The poor gas reaction effect reduces the deposition rate of the film.

[0006] 3. Patent document CN101333653B discloses a plasma chemical vapor deposition method that can avoid the generation of bag-like defects. This vapor deposition method cannot control and adjust the flow rate and pressure of the reaction gas, the degree of plasma excitation is not thorough, and the stability of the plasma cannot be guaranteed.

[0007] 4. Patent document CN103255388B discloses a plasma chemical vapor deposition method for a phosphate silicon glass film. The vapor deposition method cannot control the pulse duration of the reaction gas. If the pulse duration is not stable, it is easy to cause excessive saturation of the surface of the phosphate silicon glass, resulting in poor film deposition effect. Summary of the invention

[0008] The object of the present invention is to provide a vapor deposition method for increasing the voltage of SCR products, so as to solve the problems raised in the above background technology.

[0009] To achieve the above objectives, the present invention provides the following technical solutions: a vapor deposition method for increasing the voltage of SCR products, comprising the following steps: S1, carrier pretreatment; S2, catalyst precursor gas preparation; S3, conductive layer vapor deposition; S4, post-deposition treatment.

[0010] Preferably, the carrier pretreatment steps are as follows: (1) carrier preparation; (2) grinding and polishing; (3) cleaning; (4) drying; (5) smoothness detection.

[0011] Preferably, the steps of vapor deposition of the conductive layer are as follows: (1) introducing air into the coating equipment; (2) supplying power with a pulse power supply; (3) gas ionization coating; and (4) cleaning of by-products.

[0012] Preferably, the post-deposition processing steps are as follows: (1) deposition heat treatment; (2) post-processing; (3) quality inspection.

[0013] Preferably, the step (1) carrier preparation: selecting a thyristor cathode sheet to prepare for subsequent processing; step (2) grinding and polishing: grinding and polishing the cathode sheet to remove burrs and unevenness on the edge of the cathode sheet while ensuring the smoothness of the surface; step (3) cleaning: placing the ground and polished thyristor cathode sheet into an ultrasonic cleaning machine for cleaning to remove dirt and impurities on the surface, and the cleaning time is 2 minutes to 5 minutes; step (4) drying: drying in an oven or a dryer, the drying temperature is controlled at 110°C to 120°C, and the drying time is 5 minutes to 7 minutes; step (5) smoothness detection: using a surface smoothness tester to detect the dried cathode sheet to check the surface smoothness.

[0014] Preferably, the catalyst precursor gas preparation step is as follows: carbon tetrafluoride gas is mixed with oxygen or hydrogen to generate tetrafluoromethane gas through redox reaction, and the prepared tetrafluoromethane gas is stored in a sealed storage tank.

[0015] Preferably, the step (1) of introducing air into the coating equipment: placing the pretreated cathode sheet on the substrate electrode in the reaction chamber of the vapor deposition equipment, introducing tetrafluoromethane precursor gas into the reaction chamber after the coating equipment is sealed, and controlling the pressure of the introduced reaction gas to be 50Pa to 2000Pa for 20s to 50s, so that the gas is fully diffused on the surface of the substrate electrode; the step (2) of supplying power by a pulse power supply: the pulse power supply adopts a high-frequency 50MHz to 400MHz alternating current, and transmits the electric energy to the substrate electrode in the reaction chamber through a matching network, so as to provide radio frequency or microwave energy to excite and maintain plasma; the step (3) of gas ionization coating: in the plasma The high-energy electrons collide with the fluorine-containing precursor molecules, causing the molecules near the surface of the substrate electrode to be excited and ionized, generating fluorine free radicals and other active species. The formed carbon tetrafluoride gas then participates in the chemical reaction and promotes the occurrence of the chemical reaction. The substrate electrode deposition temperature is maintained at 300°C to 600°C, and the ionization time is 10s to 25s, thereby forming a high-quality solid film at a relatively low temperature; step (4) by-product cleaning: the required film generated by the gas reaction is attached to the surface of the cathode sheet, and other by-products will detach from the surface of the cathode sheet and diffuse in the gas cavity. The vacuum pump draws the generated carbon tetrafluoride gas and other gases out of the reaction chamber. The vacuum pumping time is 40s.

[0016] Preferably, the step (1) is a deposition heat treatment: after the deposition is completed, the substrate coated with the conductive coating is slowly heated to the required heat treatment temperature to promote the crystallization of the metal in the coating and the improvement of the catalytic activity, the heat treatment temperature is controlled at 300°C to 1000°C, and the heat treatment is kept for 2min to 8min, so that the atoms or molecules in the coating have sufficient time to rearrange, diffuse or chemically react; the step (2) is a post-treatment: after the heat treatment is completed, the substrate is slowly cooled to room temperature, and the conductive coating is passivated to improve its stability and catalytic performance; the step (3) is a quality inspection: after the post-treatment is completed, the conductive coating is subjected to a conductivity test, surface morphology observation, structural analysis and environmental stability test to ensure that it meets the expected conductivity and stability requirements.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] 1. The present invention enhances the excitation degree of plasma. RF power is the main energy source for exciting plasma. Increasing RF power can increase the density and temperature of plasma. Increasing voltage can enhance the excitation degree of plasma, improve the efficiency of chemical reaction and the rate of thin film deposition, and achieve effective chemical reaction without significantly increasing the temperature of the substrate electrode. A more uniform electric field distribution is generated in the reaction chamber, thereby improving the uniformity of plasma, achieving uniform, rapid and high-quality deposition of thin films, and improving the voltage performance of SCR products.

[0019] 2. The present invention replaces the DC power supply with a pulse power supply. The pulse power supply can provide high power in a short time to generate high-density plasma in the reaction gas. The high-density plasma can react with the surface of the substrate electrode more effectively, which is helpful to achieve more uniform film deposition on the cathode sheet, improve the deposition rate and film quality. The pulse power supply can complete the deposition process in a short time, reduce energy waste and reduce the generation of by-products, which is beneficial to environmental protection. The pulse power supply can improve the stability and uniformity of the plasma, thereby improving the voltage and deposition effect.

[0020] 3. The present invention can control the density and stability of plasma by adjusting the reaction gas flow and pressure, thereby improving the voltage and deposition rate. The gas flow and pressure have an important influence on the excitation of plasma and the thin film deposition process. Selecting tetrafluoromethane gas with high ionization energy can improve the excitation degree of plasma. Generating carbon tetrafluoride gas can provide high-density fluoride ions, which helps to enhance the plasma excitation and thin film deposition process, and further improves the voltage performance of the SCR product.

[0021] 4. The present invention adjusts the reaction gas pulse duration and the substrate electrode operating temperature. Increasing the precursor pulse time can increase the adsorption amount of the precursor on the cathode surface, and prevent the pulse time from being too long, which may lead to excessive saturation of the precursor on the cathode surface. The plasma activity promotes the chemical reaction, which can reduce the reaction temperature, so that the entire process can be carried out under low temperature conditions. Increasing the substrate electrode temperature can promote the chemical reaction of the precursor reaction gas on the cathode surface, thereby increasing the reaction chance and deposition rate, and improving the voltage performance of the product. The plasma enhanced chemical vapor deposition method is used in combination with the carrier pretreatment and deposition post-treatment process steps to achieve the best SCR product voltage performance improvement effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The vapor deposition process flow chart of the present invention;

[0023] Figure 2 It is a schematic diagram of the influence of the vapor deposition factors on the conductive properties of the film of the present invention. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] In the description of the present invention, it should be noted that the terms "upper", "lower", "inner", "outer", "front end", "rear end", "two ends", "one end", "the other end" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0026] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection or a movable connection, or a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0027] Example 1, an embodiment provided by the present invention: a vapor deposition method for increasing the voltage of SCR products, comprising the following steps: S1, carrier pretreatment; S2, catalyst precursor gas preparation; S3, conductive layer vapor deposition; S4, post-deposition treatment.

[0028] The carrier pretreatment steps are as follows: Step (1) Carrier preparation: Select a thyristor cathode sheet to prepare for subsequent processing; Step (2) Grinding and polishing: Grind and polish the cathode sheet to remove burrs and unevenness on the edge of the cathode sheet while ensuring the smoothness of the surface; Step (3) Cleaning: Put the ground and polished thyristor cathode sheet into an ultrasonic cleaning machine for cleaning to remove dirt and impurities on the surface, and the cleaning time is 2 minutes; Step (4) Drying: Use an oven or a dryer to dry, the drying temperature is controlled at 110°C, and the drying time is 5 minutes; Step (5) Smoothness detection: Use a surface smoothness tester to detect the dried cathode sheet to check the surface smoothness.

[0029] The steps for preparing the catalyst precursor gas are as follows: carbon tetrafluoride gas is mixed with oxygen or hydrogen, tetrafluoromethane gas is generated through an oxidation-reduction reaction, and the prepared tetrafluoromethane gas is stored in a sealed storage tank.

[0030] The steps of vapor deposition of the conductive layer are as follows: Step (1) Air introduction of the coating equipment: The pretreated cathode sheet is placed on the substrate electrode in the reaction chamber of the vapor deposition equipment. After the coating equipment is sealed, tetrafluoromethane precursor gas is introduced into the reaction chamber. The reaction gas pressure is controlled at 500 Pa for 30 seconds, and the gas is fully diffused on the surface of the substrate electrode; Step (2) Pulse power supply: The pulse power supply uses a high-frequency 50MHz alternating current to transmit electrical energy to the substrate electrode in the reaction chamber through a matching network to provide radio frequency or microwave energy to excite and maintain plasma; Step (3) Gas ionization coating: In the plasma The high-energy electrons collide with the fluorine-containing precursor molecules, causing the molecules near the surface of the substrate electrode to be excited and ionized, generating fluorine free radicals and other active species. The formed carbon tetrafluoride gas then participates in the chemical reaction and promotes the occurrence of the chemical reaction. The substrate electrode deposition temperature is maintained at 30°C and the ionization time is 10 seconds, thereby forming a high-quality solid film at a relatively low temperature. Step (4) by-product cleaning: the required film generated by the gas reaction adheres to the surface of the cathode sheet, and other by-products will detach from the surface of the cathode sheet and diffuse in the gas cavity. The vacuum pump draws the generated carbon tetrafluoride gas and other gases out of the reaction chamber. The vacuum pumping time is 40 seconds.

[0031] The post-deposition treatment steps are as follows: Step (1) deposition heat treatment: after the deposition is completed, the substrate coated with the conductive coating is slowly heated to the required heat treatment temperature to promote the crystallization of the metal in the coating and the improvement of the catalytic activity. The heat treatment temperature is controlled at 300°C and the heat treatment is kept for 2 minutes to allow the atoms or molecules in the coating to have sufficient time to rearrange, diffuse or chemically react; Step (2) post-treatment: after the heat treatment is completed, the substrate is slowly cooled to room temperature and the conductive coating is passivated to improve its stability and catalytic performance. Step (3) quality inspection: after the post-treatment is completed, the conductive coating is subjected to conductivity test, surface morphology observation, structural analysis and environmental stability test to ensure that it meets the expected conductivity and stability requirements.

[0032] Example 2, an embodiment provided by the present invention: a vapor deposition method for increasing the voltage of SCR products, comprising the following steps: S1, carrier pretreatment; S2, catalyst precursor gas preparation; S3, conductive layer vapor deposition; S4, post-deposition treatment.

[0033] The carrier pretreatment steps are as follows: Step (1) Carrier preparation: Select a thyristor cathode sheet to prepare for subsequent processing; Step (2) Grinding and polishing: Grind and polish the cathode sheet to remove burrs and unevenness on the edge of the cathode sheet while ensuring the smoothness of the surface; Step (3) Cleaning: Put the ground and polished thyristor cathode sheet into an ultrasonic cleaning machine for cleaning to remove dirt and impurities on the surface, and the cleaning time is 2 minutes; Step (4) Drying: Use an oven or a dryer to dry, the drying temperature is controlled at 110°C, and the drying time is 5 minutes; Step (5) Smoothness detection: Use a surface smoothness tester to detect the dried cathode sheet to check the surface smoothness.

[0034] The steps for preparing the catalyst precursor gas are as follows: carbon tetrafluoride gas is mixed with oxygen or hydrogen, tetrafluoromethane gas is generated through an oxidation-reduction reaction, and the prepared tetrafluoromethane gas is stored in a sealed storage tank.

[0035] The steps of vapor deposition of the conductive layer are as follows: Step (1) Air introduction of the coating equipment: The pretreated cathode sheet is placed on the substrate electrode in the reaction chamber of the vapor deposition equipment. After the coating equipment is sealed, tetrafluoromethane precursor gas is introduced into the reaction chamber. The pressure of the introduced reaction gas is controlled at 500 Pa. The introduction time is 30 seconds, and the gas is fully diffused on the surface of the substrate electrode; Step (2) Pulse power supply: The pulse power supply uses a high-frequency 200 MHz alternating current to transmit electrical energy to the substrate electrode in the reaction chamber through a matching network to provide radio frequency or microwave energy to excite and maintain plasma; Step (3) Gas ionization coating: In the plasma The high-energy electrons collide with the fluorine-containing precursor molecules, causing the molecules near the surface of the substrate electrode to be excited and ionized, generating fluorine free radicals and other active species. The formed carbon tetrafluoride gas then participates in the chemical reaction and promotes the occurrence of the chemical reaction. The substrate electrode deposition temperature is maintained at 300°C and the ionization time is 10 seconds, thereby forming a high-quality solid film at a relatively low temperature. Step (4) by-product cleaning: the required film generated by the gas reaction adheres to the surface of the cathode sheet, and other by-products will detach from the surface of the cathode sheet and diffuse in the gas cavity. The vacuum pump draws the generated carbon tetrafluoride gas and other gases out of the reaction chamber. The vacuum pumping time is 40 seconds.

[0036] The post-deposition treatment steps are as follows: Step (1) deposition heat treatment: after the deposition is completed, the substrate coated with the conductive coating is slowly heated to the required heat treatment temperature to promote the crystallization of the metal in the coating and the improvement of the catalytic activity. The heat treatment temperature is controlled at 300°C and the heat treatment is kept for 2 minutes to allow the atoms or molecules in the coating to have sufficient time to rearrange, diffuse or chemically react; Step (2) post-treatment: after the heat treatment is completed, the substrate is slowly cooled to room temperature and the conductive coating is passivated to improve its stability and catalytic performance. Step (3) quality inspection: after the post-treatment is completed, the conductive coating is subjected to conductivity test, surface morphology observation, structural analysis and environmental stability test to ensure that it meets the expected conductivity and stability requirements.

[0037] Depend on Figure 2 It can be seen that when the gas injection pressure, gas injection time, substrate electrode operating temperature and time are consistent, the greater the pulse power frequency, the higher the conductivity of the deposited film.

[0038] Embodiment 3, an embodiment provided by the present invention: a vapor deposition method for increasing the voltage of SCR products, comprising the following steps: S1, carrier pretreatment; S2, catalyst precursor gas preparation; S3, conductive layer vapor deposition; S4, post-deposition treatment.

[0039] The carrier pretreatment steps are as follows: Step (1) Carrier preparation: Select a thyristor rectifier cathode sheet to prepare for subsequent processing; Step (2) Grinding and polishing: Grind and polish the cathode sheet to remove burrs and unevenness on the edge of the cathode sheet while ensuring the smoothness of the surface; Step (3) Cleaning: Put the ground and polished thyristor rectifier cathode sheet into an ultrasonic cleaning machine for cleaning to remove dirt and impurities on the surface, and the cleaning time is 5 minutes; Step (4) Drying: Use an oven or a dryer to dry, the drying temperature is controlled at 120°C, and the drying time is 7 minutes; Step (5) Smoothness detection: Use a surface smoothness tester to detect the dried cathode sheet to check the surface smoothness.

[0040] The steps for preparing the catalyst precursor gas are as follows: carbon tetrafluoride gas is mixed with oxygen or hydrogen, tetrafluoromethane gas is generated through an oxidation-reduction reaction, and the prepared tetrafluoromethane gas is stored in a sealed storage tank.

[0041] The steps of vapor deposition of the conductive layer are as follows: Step (1) Air introduction of the coating equipment: The pretreated cathode sheet is placed on the substrate electrode in the reaction chamber of the vapor deposition equipment. After the coating equipment is sealed, tetrafluoromethane precursor gas is introduced into the reaction chamber. The reaction gas pressure is controlled at 50 Pa for 40 seconds, and the gas is fully diffused on the surface of the substrate electrode; Step (2) Pulse power supply: The pulse power supply uses a high-frequency 100 MHz alternating current to transmit electrical energy to the substrate electrode in the reaction chamber through a matching network to provide radio frequency or microwave energy to excite and maintain plasma; Step (3) Gas ionization coating: The plasma The high-energy electrons collide with the fluorine-containing precursor molecules, causing the molecules near the surface of the substrate electrode to be excited and ionized, generating fluorine free radicals and other active species. The formed carbon tetrafluoride gas then participates in the chemical reaction and promotes the occurrence of the chemical reaction. The substrate electrode deposition temperature is maintained at 600°C and the ionization time is 25 seconds, thereby forming a high-quality solid film at a relatively low temperature. Step (4) by-product cleaning: the required film generated by the gas reaction adheres to the surface of the cathode sheet, and other by-products will detach from the surface of the cathode sheet and diffuse in the gas cavity. The vacuum pump draws the generated carbon tetrafluoride gas and other gases out of the reaction chamber. The vacuum pumping time is 40 seconds.

[0042] The post-deposition treatment steps are as follows: Step (1) Deposition heat treatment: After the deposition is completed, the substrate coated with the conductive coating is slowly heated to the required heat treatment temperature to promote the crystallization of the metal in the coating and the improvement of the catalytic activity. The heat treatment temperature is controlled at 500°C and the heat treatment is kept for 8 minutes to allow the atoms or molecules in the coating to have sufficient time to rearrange, diffuse or chemically react; Step (2) Post-treatment: After the heat treatment is completed, the substrate is slowly cooled to room temperature and the conductive coating is passivated to improve its stability and catalytic performance. Step (3) Quality inspection: After the post-treatment is completed, the conductive coating is subjected to conductivity testing, surface morphology observation, structural analysis and environmental stability testing to ensure that it meets the expected conductivity and stability requirements.

[0043] Embodiment 4, an embodiment provided by the present invention: a vapor deposition method for increasing the voltage of SCR products, comprising the following steps: S1, carrier pretreatment; S2, catalyst precursor gas preparation; S3, conductive layer vapor deposition; S4, post-deposition treatment.

[0044] The carrier pretreatment steps are as follows: Step (1) Carrier preparation: Select a thyristor rectifier cathode sheet to prepare for subsequent processing; Step (2) Grinding and polishing: Grind and polish the cathode sheet to remove burrs and unevenness on the edge of the cathode sheet while ensuring the smoothness of the surface; Step (3) Cleaning: Put the ground and polished thyristor rectifier cathode sheet into an ultrasonic cleaning machine for cleaning to remove dirt and impurities on the surface, and the cleaning time is 5 minutes; Step (4) Drying: Use an oven or a dryer to dry, the drying temperature is controlled at 120°C, and the drying time is 7 minutes; Step (5) Smoothness detection: Use a surface smoothness tester to detect the dried cathode sheet to check the surface smoothness.

[0045] The steps for preparing the catalyst precursor gas are as follows: carbon tetrafluoride gas is mixed with oxygen or hydrogen, tetrafluoromethane gas is generated through an oxidation-reduction reaction, and the prepared tetrafluoromethane gas is stored in a sealed storage tank.

[0046] The steps of vapor deposition of the conductive layer are as follows: Step (1) Air introduction of the coating equipment: The pretreated cathode sheet is placed on the substrate electrode in the reaction chamber of the vapor deposition equipment. After the coating equipment is sealed, tetrafluoromethane precursor gas is introduced into the reaction chamber. The pressure of the introduced reaction gas is controlled at 1000 Pa. The introduction time is 40 seconds, and the gas is fully diffused on the surface of the substrate electrode; Step (2) Pulse power supply: The pulse power supply uses a high-frequency 100MHz alternating current to transmit electrical energy to the substrate electrode in the reaction chamber through a matching network to provide radio frequency or microwave energy to excite and maintain plasma; Step (3) Gas ionization coating: In the plasma The high-energy electrons collide with the fluorine-containing precursor molecules, causing the molecules near the surface of the substrate electrode to be excited and ionized, generating fluorine free radicals and other active species. The formed carbon tetrafluoride gas then participates in the chemical reaction and promotes the occurrence of the chemical reaction. The substrate electrode deposition temperature is maintained at 600°C and the ionization time is 25 seconds, thereby forming a high-quality solid film at a relatively low temperature. Step (4) by-product cleaning: the required film generated by the gas reaction adheres to the surface of the cathode sheet, and other by-products will detach from the surface of the cathode sheet and diffuse in the gas cavity. The vacuum pump draws the generated carbon tetrafluoride gas and other gases out of the reaction chamber. The vacuum pumping time is 40 seconds.

[0047] The post-deposition treatment steps are as follows: Step (1) Deposition heat treatment: After the deposition is completed, the substrate coated with the conductive coating is slowly heated to the required heat treatment temperature to promote the crystallization of the metal in the coating and the improvement of the catalytic activity. The heat treatment temperature is controlled at 500°C and the heat treatment is kept for 8 minutes to allow the atoms or molecules in the coating to have sufficient time to rearrange, diffuse or chemically react; Step (2) Post-treatment: After the heat treatment is completed, the substrate is slowly cooled to room temperature and the conductive coating is passivated to improve its stability and catalytic performance. Step (3) Quality inspection: After the post-treatment is completed, the conductive coating is subjected to conductivity testing, surface morphology observation, structural analysis and environmental stability testing to ensure that it meets the expected conductivity and stability requirements.

[0048] Depend on Figure 2 It can be seen that when the pulse power frequency, gas introduction time, substrate electrode operating temperature and time are consistent, the greater the gas introduction pressure, the higher the conductivity of the deposited film.

[0049] Example 5, an embodiment provided by the present invention: a vapor deposition method for increasing the voltage of SCR products, comprising the following steps: S1, carrier pretreatment; S2, catalyst precursor gas preparation; S3, conductive layer vapor deposition; S4, post-deposition treatment.

[0050] The carrier pretreatment steps are as follows: Step (1) Carrier preparation: Select a thyristor rectifier cathode sheet to prepare for subsequent processing; Step (2) Grinding and polishing: Grind and polish the cathode sheet to remove burrs and unevenness on the edge of the cathode sheet while ensuring the smoothness of the surface; Step (3) Cleaning: Put the ground and polished thyristor rectifier cathode sheet into an ultrasonic cleaning machine for cleaning to remove dirt and impurities on the surface, and the cleaning time is 5 minutes; Step (4) Drying: Use an oven or a dryer to dry, the drying temperature is controlled at 120°C, and the drying time is 7 minutes; Step (5) Smoothness detection: Use a surface smoothness tester to detect the dried cathode sheet to check the surface smoothness.

[0051] The steps for preparing the catalyst precursor gas are as follows: carbon tetrafluoride gas is mixed with oxygen or hydrogen, tetrafluoromethane gas is generated through an oxidation-reduction reaction, and the prepared tetrafluoromethane gas is stored in a sealed storage tank.

[0052] The steps of vapor deposition of the conductive layer are as follows: Step (1) Air introduction of the coating equipment: The pretreated cathode sheet is placed on the substrate electrode in the reaction chamber of the vapor deposition equipment. After the coating equipment is sealed, tetrafluoromethane precursor gas is introduced into the reaction chamber. The reaction gas pressure is controlled at 1000 Pa for 30 seconds, and the gas is fully diffused on the surface of the substrate electrode; Step (2) Pulse power supply: The pulse power supply uses a high-frequency 300MHz alternating current to transmit electrical energy to the substrate electrode in the reaction chamber through a matching network to provide radio frequency or microwave energy to excite and maintain plasma; Step (3) Gas ionization coating: In the plasma The high-energy electrons collide with the fluorine-containing precursor molecules, causing the molecules near the surface of the substrate electrode to be excited and ionized, generating fluorine free radicals and other active species. The formed carbon tetrafluoride gas then participates in the chemical reaction and promotes the occurrence of the chemical reaction. The substrate electrode deposition temperature is maintained at 300°C and the ionization time is 10 seconds, thereby forming a high-quality solid film at a relatively low temperature. Step (4) by-product cleaning: the required film generated by the gas reaction adheres to the surface of the cathode sheet, and other by-products will detach from the surface of the cathode sheet and diffuse in the gas cavity. The vacuum pump draws the generated carbon tetrafluoride gas and other gases out of the reaction chamber. The vacuum pumping time is 40 seconds.

[0053] The post-deposition treatment steps are as follows: Step (1) deposition heat treatment: after the deposition is completed, the substrate coated with the conductive coating is slowly heated to the required heat treatment temperature to promote the crystallization of the metal in the coating and the improvement of the catalytic activity. The heat treatment temperature is controlled at 300°C and the heat treatment is kept for 2 minutes to allow the atoms or molecules in the coating to have sufficient time to rearrange, diffuse or chemically react; Step (2) post-treatment: after the heat treatment is completed, the substrate is slowly cooled to room temperature and the conductive coating is passivated to improve its stability and catalytic performance. Step (3) quality inspection: after the post-treatment is completed, the conductive coating is subjected to conductivity test, surface morphology observation, structural analysis and environmental stability test to ensure that it meets the expected conductivity and stability requirements.

[0054] Example 6, an embodiment provided by the present invention: a vapor deposition method for increasing the voltage of SCR products, comprising the following steps: S1, carrier pretreatment; S2, catalyst precursor gas preparation; S3, conductive layer vapor deposition; S4, post-deposition treatment.

[0055] The carrier pretreatment steps are as follows: Step (1) Carrier preparation: Select a thyristor rectifier cathode sheet to prepare for subsequent processing; Step (2) Grinding and polishing: Grind and polish the cathode sheet to remove burrs and unevenness on the edge of the cathode sheet while ensuring the smoothness of the surface; Step (3) Cleaning: Put the ground and polished thyristor rectifier cathode sheet into an ultrasonic cleaning machine for cleaning to remove dirt and impurities on the surface, and the cleaning time is 5 minutes; Step (4) Drying: Use an oven or a dryer to dry, the drying temperature is controlled at 120°C, and the drying time is 7 minutes; Step (5) Smoothness detection: Use a surface smoothness tester to detect the dried cathode sheet to check the surface smoothness.

[0056] The steps for preparing the catalyst precursor gas are as follows: carbon tetrafluoride gas is mixed with oxygen or hydrogen, tetrafluoromethane gas is generated through an oxidation-reduction reaction, and the prepared tetrafluoromethane gas is stored in a sealed storage tank.

[0057] The steps of vapor deposition of the conductive layer are as follows: Step (1) Air introduction of the coating equipment: The pretreated cathode sheet is placed on the substrate electrode in the reaction chamber of the vapor deposition equipment. After the coating equipment is sealed, tetrafluoromethane precursor gas is introduced into the reaction chamber. The reaction gas pressure is controlled at 1000 Pa for 30 seconds, and the gas is fully diffused on the surface of the substrate electrode; Step (2) Pulse power supply: The pulse power supply uses a high-frequency 300MHz alternating current to transmit electrical energy to the substrate electrode in the reaction chamber through a matching network to provide radio frequency or microwave energy to excite and maintain plasma; Step (3) Gas ionization coating: In the plasma The high-energy electrons collide with the fluorine-containing precursor molecules, causing the molecules near the surface of the substrate electrode to be excited and ionized, generating fluorine free radicals and other active species. The formed carbon tetrafluoride gas then participates in the chemical reaction and promotes the occurrence of the chemical reaction. The substrate electrode deposition temperature is maintained at 450°C and the ionization time is 10 seconds, thereby forming a high-quality solid film at a relatively low temperature. Step (4) by-product cleaning: the required film generated by the gas reaction adheres to the surface of the cathode sheet, and other by-products will detach from the surface of the cathode sheet and diffuse in the gas cavity. The vacuum pump draws the generated carbon tetrafluoride gas and other gases out of the reaction chamber. The vacuum pumping time is 40 seconds.

[0058] The post-deposition treatment steps are as follows: Step (1) deposition heat treatment: after the deposition is completed, the substrate coated with the conductive coating is slowly heated to the required heat treatment temperature to promote the crystallization of the metal in the coating and the improvement of the catalytic activity. The heat treatment temperature is controlled at 300°C and the heat treatment is kept for 2 minutes to allow the atoms or molecules in the coating to have sufficient time to rearrange, diffuse or chemically react; Step (2) post-treatment: after the heat treatment is completed, the substrate is slowly cooled to room temperature and the conductive coating is passivated to improve its stability and catalytic performance. Step (3) quality inspection: after the post-treatment is completed, the conductive coating is subjected to conductivity test, surface morphology observation, structural analysis and environmental stability test to ensure that it meets the expected conductivity and stability requirements.

[0059] Depend on Figure 2 It can be seen that when the gas injection pressure, gas injection time, pulse power frequency and substrate electrode working time are consistent, the higher the substrate electrode working temperature, the higher the conductivity of the deposited film.

[0060] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A vapor deposition method for increasing the voltage of SCR products, Features: The method comprises the following steps: S1, carrier pretreatment; S2, catalyst precursor gas preparation; S3, conductive layer vapor deposition; S4, post-deposition treatment; The steps of vapor deposition of the conductive layer are as follows: (1) introducing gas into the coating equipment; (2) supplying power with a pulse power supply; (3) gas ionization coating; (4) cleaning of by-products; The step (1) of introducing gas into the coating equipment: placing the pretreated cathode sheet on the substrate electrode in the reaction chamber of the vapor deposition equipment, and introducing tetrafluoromethane precursor gas into the reaction chamber after the coating equipment is sealed, wherein the gas pressure of the introduced reaction gas is controlled at 50Pa to 2000Pa, and the introduction time is 20s to 50s, and the gas is fully diffused on the surface of the substrate electrode; the step (2) of supplying power by a pulse power supply: the pulse power supply adopts a high frequency 50MHz to 400MHz alternating current, and transmits the electric energy to the substrate electrode in the reaction chamber through a matching network, so as to provide radio frequency or microwave energy to excite and maintain plasma; the step (3) of gas ionization coating: the high frequency in the plasma The energetic electrons collide with the fluorine-containing precursor molecules, causing the molecules near the surface of the substrate electrode to be excited and ionized, generating fluorine free radicals and other active species. The formed carbon tetrafluoride gas then participates in the chemical reaction and promotes the occurrence of the chemical reaction. The substrate electrode deposition temperature is maintained at 300°C to 600°C, and the ionization time is 10s to 25s, thereby forming a high-quality solid film at a relatively low temperature. Step (4) by-product cleaning: the required film generated by the gas reaction adheres to the surface of the cathode sheet, and other by-products will detach from the surface of the cathode sheet and diffuse in the gas cavity. The vacuum pump draws the generated carbon tetrafluoride gas and other gases out of the reaction chamber. The vacuum pumping time is 40s.

2. A vapor deposition method for increasing the voltage of an SCR product according to claim 1, Features: The carrier pretreatment steps are as follows: (1) carrier preparation; (2) grinding and polishing; (3) cleaning; (4) drying; and (5) smoothness detection.

3. A vapor deposition method for increasing the voltage of an SCR product according to claim 1, Features: The post-deposition processing steps are as follows: (1) deposition heat treatment; (2) post-processing; (3) quality inspection.

4. A vapor deposition method for increasing the voltage of an SCR product according to claim 2, Features: The step (1) carrier preparation: selecting a thyristor cathode sheet to prepare for subsequent processing; step (2) grinding and polishing: grinding and polishing the cathode sheet to remove burrs and unevenness on the edge of the cathode sheet while ensuring the smoothness of the surface; step (3) cleaning: placing the ground and polished thyristor cathode sheet into an ultrasonic cleaning machine for cleaning to remove dirt and impurities on the surface, and the cleaning time is 2 minutes to 5 minutes; step (4) drying: drying in an oven or a dryer, the drying temperature is controlled at 110° C. to 120° C., and the drying time is 5 minutes to 7 minutes; step (5) smoothness detection: using a surface smoothness tester to detect the dried cathode sheet to check the surface smoothness.

5. A vapor deposition method for increasing the voltage of an SCR product according to claim 1, Features: The catalyst precursor gas preparation steps are as follows: carbon tetrafluoride gas is mixed with oxygen or hydrogen to generate tetrafluoromethane gas through redox reaction, and the prepared tetrafluoromethane gas is stored in a sealed storage tank.

6. A vapor deposition method for increasing the voltage of an SCR product according to claim 3, Features: The step (1) of deposition heat treatment: after the deposition is completed, the substrate coated with the conductive coating is slowly heated to the required heat treatment temperature to promote the crystallization of the metal in the coating and the improvement of the catalytic activity. The heat treatment temperature is controlled at 300°C to 1000°C, and the heat treatment is kept for 2min to 8min, so that the atoms or molecules in the coating have sufficient time to rearrange, diffuse or chemically react. The step (2) of post-treatment: after the heat treatment is completed, the substrate is slowly cooled to room temperature, and the conductive coating is passivated to improve its stability and catalytic performance. The step (3) of quality inspection: after the post-treatment is completed, the conductive coating is subjected to conductivity test, surface morphology observation, structural analysis and environmental stability test to ensure that it meets the expected conductivity and stability requirements.