A method for preparing durable antistatic polyester fabric
Through natural eutectic solvent activation and reactive biomass ink cross-linking technology, the problems of poor hydrophilicity and easy generation of static electricity in polyester fabrics are solved, and the durable antistatic performance and environmental protection are improved.
Patent Information
- Application Number
- CN202410895318.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Due to poor hydrophilicity, existing polyester fabrics have poor moisture absorption, poor moisture permeability, and easy generation of static electricity, which poses safety risks. Moreover, the commonly used modification methods have problems such as poor durability, high cost, and insufficient environmental protection.
The polyester fabric is surface-activated using a natural eutectic solvent, and after padding with a hydroxypropyltrimethylammonium chloride chitosan solution, the reactive biomass antistatic ink is sprayed through atomization to perform a cross-linking reaction. Catalyst and plasma treatment to form durable antistatic polyester fabric.
It significantly improves the hydrophilicity and antistatic properties, durability and safety of polyester fabrics, reduces water consumption and environmental burden, and meets the development requirements of the green textile industry.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional modified polyester fabrics and relates to a method for preparing durable antistatic polyester fabrics. Background Art
[0002] Polyester (Polyethlene terephthalate, PET) fiber is the largest synthetic fiber variety, accounting for about 90% of the total synthetic fiber production. PET fiber is widely used in the production of clothing fabrics and industrial products due to its excellent properties such as durability, not easy to deform, easy to wash and quick drying. However, due to the lack of hydrophilic groups in its polyester molecular structure, its moisture absorption and moisture permeability are poor, and the standard moisture regain is only 0.4%~0.5%. Even at 100% relative humidity, the moisture absorption rate is only 0.6%~0.8%, which seriously affects the comfort of polyester clothing or decorations. In addition, for polyester fabrics, static electricity is easily generated in a dry environment due to poor hydrophilicity, which poses a safety hazard. In order to solve this problem, various means are usually taken to give the fabric surface a certain degree of hydrophilicity, thereby improving its conductivity and achieving the purpose of improving antistatic properties.
[0003] In order to improve the hydrophilicity of polyester fibers, the main methods adopted by the textile industry include surface morphology and structure modification, adsorption and fixation of hydrophilic finishing agents, and surface grafting modification, etc. Although these methods have improved the hydrophilicity of polyester fibers to a certain extent, there are still some significant defects.
[0004] Although surface morphology modification can improve the hydrophilicity of polyester by giving the fiber a special-shaped cross-section or an uneven surface structure through various physical or chemical means, increasing the water infiltration and contact area on the fiber surface, this puts higher demands on the production process of polyester, making weaving difficult, inefficient, cost-intensive, and prone to producing hair. Although it can indirectly improve the hydrophilicity of the fiber assembly, it does not significantly improve the hydrophilicity of polyester itself.
[0005] The most common and feasible method of finishing with a hydrophilic finishing agent is to improve the hydrophilicity and antistatic properties of fibers. For example, Reference 1 (Study on Process Parameters of Polyester Hydrophilic Softening Finishing, Dyeing and Finishing Technology 34 (2012) 12-14) used polyester polyether silicone ternary block copolymer finishing agent DP-9993 to finish polyester fabric. When the finishing process was 15 g / L finishing agent, two dips and two rolls (rolling liquid rate 70%~80%) - pre-baking (110℃, 180s) - baking (180℃, 60s), the radial hair effect of the polyester fabric increased from 12.5cm to 20cm, and the static half-life decreased to 0.54s; however, there are the following problems: (1) poor durability; (2) the hydrophilic finishing agent will remain on the fabric, which may pose a safety hazard to the human body. Reference 2 (Synthesis and Application of Polyester Hydrophilic Finishing Agent LS, Dyeing and Finishing Technology 34 (2012) 45-49) uses phthalic anhydride and polyethylene glycol to synthesize polyester polyether hydrophilic agent LS, which can reduce the wetting time of polyester fabric to 4.05s, and recover to 25.81s after 5 washes. However, it has problems such as high water and energy consumption and poor durability.
[0006] Surface grafting modification is a method that can obtain relatively long-lasting and effective hydrophilic properties. For example, Reference 3 (Effect of plasma grafting reaction on hydrophilic properties of polyester fabrics, Journal of Textile Research 31 (2010) 74-78) used polymerized monomers and argon plasma to modify polyester fabrics. The surface wetting time was 2.9s and the water diffusion rate was 7.2mm / s. However, after 10 washes, the wetting time and water diffusion rate decreased by 41.3% and 41.7%, respectively. However, this type of hydrophilic finishing technology still has the following problems: (1) Most commonly used hydrophilic agents are synthetic hydrophilic agents, and their safety and ecological properties need to be further improved; (2) The environmental protection of commonly used cross-linking agents is also worthy of attention, which does not meet the development requirements of the green textile industry; (3) The textile processing method is still commonly treated by immersion, which is not only inefficient, but also produces a large amount of wastewater, increasing the environmental burden.
[0007] Therefore, it is of great significance to study a method for preparing a durable antistatic polyester fabric to solve the problems existing in the prior art. Summary of the invention
[0008] The purpose of the invention is to solve the problems existing in the prior art and provide a method for preparing a durable antistatic polyester fabric.
[0009] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0010] A method for preparing a durable antistatic polyester fabric comprises the following steps: firstly, performing a surface activation treatment on the polyester fabric, and then padding the polyester fabric after the surface activation treatment with a hydroxypropyl trimethyl ammonium chloride chitosan (CAS: 9012-76-4) solution, wherein the hydroxypropyl trimethyl ammonium chloride chitosan is a biomass derivative cation, which can reduce the repulsive force between the subsequent surface anionic charge of the polyester and butane tetracarboxylic acid, citric acid, catechins, and caffeic acid, and reduce the distance between molecules, thereby promoting the subsequent cross-linking effect, and then using a reactive biomass antistatic ink to spray the polyester fabric after padding with the hydroxypropyl trimethyl ammonium chloride chitosan solution, and then performing a catalytic cross-linking reaction under a baking condition, and then rinsing with water after the reaction, and finally performing a plasma treatment on the polyester fabric after the reaction, so as to prepare the durable antistatic polyester fabric;
[0011] The method for surface activation treatment of polyester fabric is as follows: placing the polyester fabric in a natural eutectic solvent and treating it at a temperature of 60-80°C for 30-60 minutes, locally etching the surface of the polyester fabric, breaking part of the surface macromolecules, thereby increasing the reactive hydroxyl content on the surface of the fabric;
[0012] The natural eutectic solvent is composed of a hydrogen bond donor and a hydrogen bond acceptor, and the molar ratio of the hydrogen bond donor to the hydrogen bond acceptor is 0.5~4:1;
[0013] Based on the hydroxyl content and strength loss of PET surface, a high ratio of hydrogen bond acceptors to hydrogen bond donors in natural eutectic solvents, too high a treatment temperature, or too long a treatment time will cause serious degradation of polyester fibers, affecting the quality of the final product when used.
[0014] The reactive biomass antistatic ink is prepared by mixing chitosan, catechin, caffeic acid, tea saponin, citric acid, butane tetracarboxylic acid and sodium phytate and dissolving them in water. Citric acid and caffeic acid provide acidity for chitosan to dissolve it, so that all components can be dissolved in water.
[0015] As the preferred technical solution:
[0016] In the method for preparing a durable antistatic polyester fabric as described above, the mass volume ratio of the polyester fabric to the natural eutectic solvent is 1 g:100 mL.
[0017] In the method for preparing a durable antistatic polyester fabric as described above, the hydrogen bond donor is D-glucose, D-fructose, citric acid, L-malic acid, xylitol or menthol, and the hydrogen bond acceptor is choline chloride, betaine or proline.
[0018] In the preparation method of a durable antistatic polyester fabric as described above, the configuration process of the reactive biomass antistatic ink is as follows: chitosan, catechin, caffeic acid, tea saponin, citric acid, butanetetracarboxylic acid (BTCA) and sodium phytate are mixed and dissolved in water, first stirred at a stirring speed of 800 rpm in a magnetic stirrer for 20 minutes, and then treated in an ultrasonic processor at a power of 100~500W for 5~20 minutes.
[0019] In the preparation method of a durable antistatic polyester fabric as described above, the mass ratio of chitosan, catechin, caffeic acid, tea saponin, citric acid, butanetetracarboxylic acid and sodium phytate is 1:2~6:2~6:4~5:6~10:6~10:8~10; and the total concentration of the reactive biomass antistatic ink is 20~50g / L.
[0020] In the method for preparing a durable antistatic polyester fabric as described above, the concentration of the hydroxypropyltrimethylammonium chloride chitosan solution is 1-5 g / L; the residual rate of the polyester fabric after surface activation treatment that is dipped in the hydroxypropyltrimethylammonium chloride chitosan solution is 50-80%.
[0021] In the method for preparing a durable antistatic polyester fabric as described above, the baking conditions are: pre-baking at 80°C for 60 minutes, and then baking at 100-140°C for 2-15 minutes.
[0022] In the method for preparing a durable antistatic polyester fabric as described above, the plasma treatment atmosphere is oxygen, the power is 5-30W, and the time is 1-3min. If the plasma treatment power is too high or the time is too long, the surface hydrophilic film will fall off, and even the strength of the polyester fabric will be lost.
[0023] The method for preparing a durable antistatic polyester fabric as described above, when not washed with soap, the peak voltage of the durable antistatic polyester fabric is 52-250V, and the static half-life is 0.2s-43s;
[0024] Compared with the case without soap washing, after 5 soap washings, the peak voltage of the durable antistatic polyester fabric changes by no more than 8%, and the static half-life changes by no more than 20%;
[0025] Compared with the case without soap washing, after 20 soap washings, the peak voltage of the durable antistatic polyester fabric changes by no more than 15% 287.5, and the static half-life changes by no more than 30%.
[0026] According to the method for preparing a durable antistatic polyester fabric, the whiteness of the durable antistatic polyester fabric is not less than 78%.
[0027] Principle of the invention:
[0028] The invention firstly adopts a natural eutectic solvent to pre-treat the polyester fabric, which can cause local etching on the surface of the polyester fabric, strengthen the contact with the local etching site of the fiber during subsequent electrostatic spraying film formation, improve the fixation fastness, and with the introduction of subsequent covalent cross-linking, the washing fastness of the hydrophilic film can be significantly improved; after the polyester fabric is pre-treated with the natural eutectic solvent, it is impregnated with a hydroxypropyl trimethyl ammonium chloride chitosan solution, and the hydroxypropyl trimethyl ammonium chloride chitosan is a biomass derivative cation, which can reduce the repulsive force between the subsequent polyester surface anionic charge and butane tetracarboxylic acid, citric acid, catechins, and caffeic acid, reduce the distance between molecules, and thus promote the subsequent cross-linking effect.
[0029] The present invention achieves excellent antistatic finishing effect by atomizing and spraying reactive biomass antistatic ink to form a crosslinked film on the surface of polyester fabric. The main components of the reactive biomass antistatic ink are chitosan, catechin, caffeic acid, tea saponin, citric acid and butane tetracarboxylic acid (BTCA), wherein chitosan and catechin are biomass antistatic components, tea saponin is a biomass dispersing stabilizer, which plays a role in stabilizing the dispersion of ink, and tea saponin has the effect of promoting wetting and penetration, which can make the ink fully spread on the activated part of the fiber surface, promote the reaction to occur fully, and help to improve hydrophilicity and durability, citric acid and butane tetracarboxylic acid have a crosslinking effect on hydroxyl groups, and caffeic acid and citric acid provide acidic conditions for the dissolution of chitosan, without the need for additional acid dissolution. After electrostatic spraying, chitosan is easy to form a film, and during the baking process, the crosslinking reaction between the crosslinking agent (citric acid and BTCA) and the polyphenol component (catechin) and the hydroxyl group on the surface of PET enhances the stability and durability of the film layer.
[0030] Among them, the reaction process of citric acid / BTCA and the hydroxyl groups on the surface of PET is a step-by-step anhydride-esterification process, that is, an anhydride is formed first, the anhydride and the hydroxyl group undergo esterification reaction, and then the second anhydride is formed, and the newly formed anhydride undergoes esterification reaction with the hydroxyl group. The present invention uses biomass sodium phytate instead of traditional sodium hypophosphite as a biomass catalyst. Since the hydrogen bonding between citric acid / BTCA molecules will limit the dehydration of carboxyl groups to anhydride, and the alkalinity of sodium phytate (pH about 11) is much higher than the weakly alkaline sodium hypophosphite (pH 7-8), it promotes the rapid generation of sodium carboxylate, that is, sodium phytate can reduce the anhydride formation temperature of BTCA from 205°C to about 180°C, thereby weakening the hydrogen bonding between molecules and promoting anhydride formation. In view of the relatively small number of hydrophilic groups on the surface of PET fibers and the complex composition of the coating formula, efficient cross-linking is very important for forming a durable film on the surface of PET fibers. The antistatic finishing of the present invention adopts the method of atomization spraying, which requires efficient film formation in a short time. Compared with dipping and padding, this method has higher requirements for reaction efficiency. If the catalyst is replaced by sodium hypophosphite, the film formation will be weak and easy to fall off. In addition, hypophosphorous acid is an inorganic salt, which is suitable for hydrophilic cellulose and can penetrate into the interior, but its affinity for hydrophobic PET is not as good as that of organic structure sodium phytate. The surface of PET is more likely to adsorb organic structure sodium phytate to catalyze the reaction, so sodium phytate is more suitable for polyester modification than sodium hypophosphite.
[0031] Under high temperature conditions, citric acid / BTCA is prone to undergo dehydration and oxidation side reactions to produce a small amount of unsaturated acid, which causes the fabric to turn yellow and affects whiteness; in addition, the unsaturated acid will react with the hydroxyl groups on some polyester fibers, reducing the cross-linking efficiency of BTCA. The present invention uses catechins and caffeic acid in combination to effectively capture oxidative products, reduce dehydration and oxidation side reactions, and thus alleviate the tendency of fabrics to turn yellow; at the same time, it protects the activated hydroxyl groups on PET and increases the reaction rate of BTCA with hydroxyl groups.
[0032] Beneficial effects:
[0033] (1) A method for preparing a durable antistatic polyester fabric of the present invention comprises the following steps: pre-treating the polyester fabric with a natural eutectic solvent and then impregnating the polyester fabric with a hydroxypropyl trimethyl ammonium chloride chitosan solution. The hydroxypropyl trimethyl ammonium chloride chitosan is a biomass derivative cation, which can reduce the repulsive force between the anionic charge on the surface of the polyester and butane tetracarboxylic acid, catechins, and caffeic acid, and reduce the distance between molecules, thereby promoting subsequent cross-linking. The tea saponin used has a penetration-promoting effect, which can enable cross-linking to fully occur at the surface etching site, thereby helping to improve hydrophilicity and durability.
[0034] (2) The method for preparing a durable antistatic polyester fabric of the present invention achieves an excellent antistatic finishing effect by atomizing and spraying reactive biomass antistatic ink to form a cross-linked film on the surface of the polyester fabric; and biomass sodium phytate is used instead of traditional sodium hypophosphite as a biomass catalyst. The sodium ions in sodium phytate can weaken the hydrogen bonding effect between BTCA molecules, reduce the anhydride and esterification temperatures, shorten the esterification time, improve the esterification efficiency, and improve the fastness;
[0035] (3) The present invention provides a method for preparing a durable antistatic polyester fabric. The chemical activator used for pre-treatment of the polyester fabric is a safe and non-toxic natural eutectic solvent. The plasma surface activation technology used after the reaction is a clean physical modification technology that can be mass-produced. The method is simple, easy to operate, and green and environmentally friendly. DETAILED DESCRIPTION
[0036] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0037] The test methods involved in the performance indicators in the embodiments and comparative examples of the present invention are as follows:
[0038] Hygroscopicity: The moisture regain of the fiber is measured by the oven drying method according to GB / T 9995-1997.
[0039] Static half-life: Determined in accordance with GBT 12703.1-2008 "Evaluation of electrostatic properties of textiles Part 1: Static voltage half-life".
[0040] Soap washing durability test: Soap washing is carried out according to the method in GB / T 3921-2008, and the moisture regain and static half-life of the fabric are tested after soap washing.
[0041] Example 1
[0042] A method for preparing a durable antistatic polyester fabric, the specific steps are as follows:
[0043] (1) The polyester fabric was placed in a natural eutectic solvent composed of L-malic acid and choline chloride at a mass volume ratio of 1 g:100 mL and surface activated at 60 °C for 30 min;
[0044] Wherein, the molar ratio of L-malic acid to choline chloride is 1:1;
[0045] (2) Dipping the polyester fabric after surface activation treatment into a 1 g / L hydroxypropyltrimethylammonium chloride chitosan (CAS: 9012-76-4) solution, and controlling the residual rate to 50%;
[0046] (3) Chitosan, catechin, caffeic acid, tea saponin, citric acid, butane tetracarboxylic acid and sodium phytate were mixed and dissolved in water, first stirred at a stirring speed of 800 rpm for 20 min in a magnetic stirrer, and then treated at a power of 150 W for 5 min in an ultrasonic processor to obtain a reactive biomass antistatic ink with a total concentration of 20 g / L;
[0047] The mass ratio of chitosan, catechin, caffeic acid, tea saponin, citric acid, butanetetracarboxylic acid and sodium phytate is 1:2:2:4:6:6:8;
[0048] (4) using a reactive biomass antistatic ink to spray the polyester fabric impregnated with the hydroxypropyltrimethylammonium chloride chitosan solution in step (2), and then pre-baking at 80° C. for 60 minutes and then baking at 100° C. for 2 minutes to perform a catalytic cross-linking reaction;
[0049] The atomization spraying process was as follows: spraying rate 5 mL / min, time 5 s, distance 30 cm from the sample;
[0050] (5) The polyester fabric after the reaction in step (4) was subjected to plasma treatment for 2 minutes in an oxygen atmosphere at a power of 20 W to obtain a durable antistatic polyester fabric.
[0051] Before soap washing, the peak voltage of the durable antistatic polyester fabric was 250V, the electrostatic half-life was 43s, and the moisture regain was 0.47±0.04%; after 5 soap washings, the peak voltage of the durable antistatic polyester fabric was 269V, the electrostatic half-life was 48.7s, and the moisture regain was 0.43±0.04%; after 20 soap washings, the peak voltage of the durable antistatic polyester fabric was 285V, the electrostatic half-life was 55.8s, and the moisture regain was 0.42%±0.03%; the whiteness of the durable antistatic polyester fabric was 78%.
[0052] Example 2
[0053] A method for preparing a durable antistatic polyester fabric, the specific steps are as follows:
[0054] (1) The polyester fabric was placed in a natural eutectic solvent composed of xylitol and choline chloride at a mass volume ratio of 1 g:100 mL and surface activated at 70 °C for 30 min;
[0055] Wherein, the molar ratio of xylitol to choline chloride is 2:1;
[0056] (2) Dipping the polyester fabric after surface activation treatment into a 2 g / L hydroxypropyltrimethylammonium chloride chitosan (CAS: 9012-76-4) solution, and controlling the residual rate to 60%;
[0057] (3) Chitosan, catechin, caffeic acid, tea saponin, citric acid, butane tetracarboxylic acid and sodium phytate were mixed and dissolved in water, first stirred at a stirring speed of 800 rpm for 20 min in a magnetic stirrer, and then treated at a power of 150 W for 5 min in an ultrasonic processor to obtain a reactive biomass antistatic ink with a total concentration of 30 g / L;
[0058] The mass ratio of chitosan, catechin, caffeic acid, tea saponin, citric acid, butanetetracarboxylic acid and sodium phytate is 1:3:3:4:6:6:8;
[0059] (4) using a reactive biomass antistatic ink to spray the polyester fabric impregnated with the hydroxypropyltrimethylammonium chloride chitosan solution in step (2), and then pre-baking at 80° C. for 60 minutes and then baking at 100° C. for 2 minutes to perform a catalytic cross-linking reaction;
[0060] The atomization spraying process was as follows: spraying rate 5 mL / min, time 5 s, distance 30 cm from the sample;
[0061] (5) The polyester fabric after the reaction in step (4) was subjected to plasma treatment in an oxygen atmosphere at a power of 10 W for 1 min to obtain a durable antistatic polyester fabric.
[0062] Before soap washing, the peak voltage of the durable antistatic polyester fabric was 221V, the electrostatic half-life was 32s, and the moisture regain was 0.63±0.04%; after 5 soap washings, the peak voltage of the durable antistatic polyester fabric was 236V, the electrostatic half-life was 35.7s, and the moisture regain was 0.55±0.04%; after 20 soap washings, the peak voltage of the durable antistatic polyester fabric was 253V, the electrostatic half-life was 40.8s, and the moisture regain was 0.42%±0.03%; the whiteness of the durable antistatic polyester fabric was 79%.
[0063] Example 3
[0064] A method for preparing a durable antistatic polyester fabric, the specific steps are as follows:
[0065] (1) The polyester fabric was placed in a natural eutectic solvent composed of xylitol and choline chloride at a mass volume ratio of 1 g:100 mL and surface activated at 70 °C for 30 min;
[0066] Wherein, the molar ratio of xylitol to choline chloride is 2:1;
[0067] (2) Dip the surface activated polyester fabric into a 3 g / L hydroxypropyltrimethylammonium chloride chitosan (CAS: 9012-76-4) solution and control the residual rate to 70%;
[0068] (3) Chitosan, catechin, caffeic acid, tea saponin, citric acid, butane tetracarboxylic acid and sodium phytate were mixed and dissolved in water, first stirred at a stirring speed of 800 rpm for 20 min in a magnetic stirrer, and then treated at a power of 150 W for 5 min in an ultrasonic processor to obtain a reactive biomass antistatic ink with a total concentration of 30 g / L;
[0069] The mass ratio of chitosan, catechin, caffeic acid, tea saponin, citric acid, butanetetracarboxylic acid and sodium phytate is 1:3:3:5:6:6:9;
[0070] (4) using a reactive biomass antistatic ink to spray the polyester fabric impregnated with the hydroxypropyltrimethylammonium chloride chitosan solution in step (2), and then pre-baking at 80° C. for 60 minutes and then baking at 100° C. for 2 minutes to perform a catalytic cross-linking reaction;
[0071] The atomization spraying process was as follows: spraying rate 5 mL / min, time 5 s, distance 30 cm from the sample;
[0072] (5) The polyester fabric after the reaction in step (4) was subjected to plasma treatment for 2 minutes in an oxygen atmosphere at a power of 20 W to obtain a durable antistatic polyester fabric.
[0073] Before soap washing, the peak voltage of the durable antistatic polyester fabric was 156V, the electrostatic half-life was 20s, and the moisture regain was 0.78±0.02%; after 5 soap washings, the peak voltage of the durable antistatic polyester fabric was 166V, the electrostatic half-life was 24s, and the moisture regain was 0.65±0.05%; after 20 soap washings, the peak voltage of the durable antistatic polyester fabric was 176V, the electrostatic half-life was 26s, and the moisture regain was 0.71±0.03%; the whiteness of the durable antistatic polyester fabric was 79%.
[0074] Example 4
[0075] A method for preparing a durable antistatic polyester fabric, the specific steps are as follows:
[0076] (1) The polyester fabric was placed in a natural eutectic solvent composed of xylitol and choline chloride at a mass volume ratio of 1 g:100 mL and surface activated at 70 °C for 30 min;
[0077] Wherein, the molar ratio of xylitol to choline chloride is 2:1;
[0078] (2) The polyester fabric after surface activation treatment was dipped into a 4 g / L hydroxypropyltrimethylammonium chloride chitosan (CAS: 9012-76-4) solution, and the rolling rate was controlled to be 70%;
[0079] (3) Chitosan, catechin, caffeic acid, tea saponin, citric acid, butane tetracarboxylic acid and sodium phytate were mixed and dissolved in water, first stirred at a stirring speed of 800 rpm for 20 min in a magnetic stirrer, and then treated at a power of 150 W for 5 min in an ultrasonic processor to obtain a reactive biomass antistatic ink with a total concentration of 30 g / L;
[0080] The mass ratio of chitosan, catechin, caffeic acid, tea saponin, citric acid, butanetetracarboxylic acid and sodium phytate is 1:3:3:5:8:8:9;
[0081] (4) using a reactive biomass antistatic ink to spray the polyester fabric impregnated with the hydroxypropyltrimethylammonium chloride chitosan solution in step (2), and then pre-baking at 80° C. for 60 minutes and then baking at 100° C. for 2 minutes to perform a catalytic cross-linking reaction;
[0082] The atomization spraying process was as follows: spraying rate 5 mL / min, time 5 s, distance 30 cm from the sample;
[0083] (5) The polyester fabric after the reaction in step (4) was subjected to plasma treatment for 2 minutes in an oxygen atmosphere at a power of 20 W to obtain a durable antistatic polyester fabric.
[0084] Before soap washing, the peak voltage of the durable antistatic polyester fabric was 69V, the electrostatic half-life was 2s, and the moisture regain was 0.82±0.04%; after 5 soap washings, the peak voltage of the durable antistatic polyester fabric was 73V, the electrostatic half-life was 2.3s, and the moisture regain was 0.75±0.03%; after 20 soap washings, the peak voltage of the durable antistatic polyester fabric was 78V, the electrostatic half-life was 2.5s, and the moisture regain was 0.78±0.03%; the whiteness of the durable antistatic polyester fabric was 80%.
[0085] Example 5
[0086] A method for preparing a durable antistatic polyester fabric, the specific steps are as follows:
[0087] (1) The polyester fabric was placed in a natural eutectic solvent composed of xylitol and choline chloride at a mass volume ratio of 1 g:100 mL and surface activated at 70 °C for 30 min;
[0088] Wherein, the molar ratio of xylitol to choline chloride is 2:1;
[0089] (2) Dipping the polyester fabric after surface activation treatment into a 5 g / L hydroxypropyltrimethylammonium chloride chitosan (CAS: 9012-76-4) solution, and controlling the residual rate to 80%;
[0090] (3) Chitosan, catechin, caffeic acid, tea saponin, citric acid, butane tetracarboxylic acid and sodium phytate were mixed and dissolved in water, first stirred at a stirring speed of 800 rpm for 20 min in a magnetic stirrer, and then treated at a power of 150 W for 5 min in an ultrasonic processor to obtain a reactive biomass antistatic ink with a total concentration of 30 g / L;
[0091] The mass ratio of chitosan, catechin, caffeic acid, tea saponin, citric acid, butanetetracarboxylic acid and sodium phytate is 1:3:3:5:8:8:9;
[0092] (4) using a reactive biomass antistatic ink to spray the polyester fabric impregnated with the hydroxypropyltrimethylammonium chloride chitosan solution in step (2), and then pre-baking at 80° C. for 60 min and then baking at 120° C. for 3 min to perform a catalytic cross-linking reaction;
[0093] The atomization spraying process was as follows: spraying rate 5 mL / min, time 5 s, distance 30 cm from the sample;
[0094] (5) The polyester fabric after the reaction in step (4) was subjected to plasma treatment for 2 minutes in an oxygen atmosphere at a power of 30 W to obtain a durable antistatic polyester fabric.
[0095] Before soap washing, the peak voltage of the durable antistatic polyester fabric was 58V, the electrostatic half-life was 1s, and the moisture regain was 0.93±0.04%; after 5 soap washings, the peak voltage of the durable antistatic polyester fabric was 62V, the electrostatic half-life was 1.2s, and the moisture regain was 0.87±0.03%; after 20 soap washings, the peak voltage of the durable antistatic polyester fabric was 72.5V, the electrostatic half-life was 1.3s, and the moisture regain was 0.88±0.02%; the whiteness of the durable antistatic polyester fabric was 80%.
[0096] Example 6
[0097] A method for preparing a durable antistatic polyester fabric, the specific steps are as follows:
[0098] (1) The polyester fabric was placed in a natural eutectic solvent composed of xylitol and choline chloride at a mass volume ratio of 1 g:100 mL and surface activated at 70 °C for 30 min;
[0099] Wherein, the molar ratio of xylitol to choline chloride is 2:1;
[0100] (2) Dipping the polyester fabric after surface activation treatment into a 5 g / L hydroxypropyltrimethylammonium chloride chitosan (CAS: 9012-76-4) solution, and controlling the residual rate to 80%;
[0101] (3) Chitosan, catechin, caffeic acid, tea saponin, citric acid, butane tetracarboxylic acid and sodium phytate were mixed and dissolved in water, first stirred at a stirring speed of 800 rpm for 20 min in a magnetic stirrer, and then treated at a power of 150 W for 5 min in an ultrasonic processor to obtain a reactive biomass antistatic ink with a total concentration of 30 g / L;
[0102] The mass ratio of chitosan, catechin, caffeic acid, tea saponin, citric acid, butanetetracarboxylic acid and sodium phytate is 1:3:3:5:8:8:10;
[0103] (4) using a reactive biomass antistatic ink to spray the polyester fabric impregnated with the hydroxypropyltrimethylammonium chloride chitosan solution in step (2), and then pre-baking at 80° C. for 60 min and then baking at 140° C. for 10 min to perform a catalytic cross-linking reaction;
[0104] The atomization spraying process was as follows: spraying rate 5 mL / min, time 5 s, distance 30 cm from the sample;
[0105] (5) The polyester fabric after the reaction in step (4) was subjected to plasma treatment for 2 minutes in an oxygen atmosphere at a power of 30 W to obtain a durable antistatic polyester fabric.
[0106] Before soap washing, the peak voltage of the durable antistatic polyester fabric was 52V, the electrostatic half-life was 0.2s, and the regain was 1.2±0.04%; after 5 soap washings, the peak voltage of the durable antistatic polyester fabric was 56V, the electrostatic half-life was 0.24s, and the regain was 1.13±0.03%; after 20 soap washings, the peak voltage of the durable antistatic polyester fabric was 59V, the electrostatic half-life was 0.26s, and the regain was 1.15±0.04%; the whiteness of the durable antistatic polyester fabric was 80%.
[0107] Comparative Example 1
[0108] A method for preparing a durable antistatic polyester fabric is basically the same as that of Example 6, except that the step (2) of impregnating the hydroxypropyltrimethylammonium chloride chitosan solution is omitted.
[0109] Before soap washing, the peak voltage of the durable antistatic polyester fabric was 422V, the static half-life was 60s, and the regain was 0.53±0.03%; after 5 soap washings, the peak voltage of the durable antistatic polyester fabric was 842V, the static half-life was 112s, and the regain was 0.45±0.04%; the whiteness of the durable antistatic polyester fabric was 75%.
[0110] By comparing Comparative Example 1 with Example 6, it can be found that the durability and antistatic properties of Comparative Example 1 are reduced, and the whiteness is reduced. This is because the padding of hydroxypropyltrimethylammonium chloride chitosan is omitted, and the hydrophilic groups on the surface of the polyester fabric after surface activation treatment are strongly negatively charged, and the repulsion to the cross-linking agent and catalyst that are negatively charged after ionization is strong, which reduces the content of the antistatic component chitosan and the polyphenol content adsorbed on the fabric, so the subsequent cross-linking reaction degree is low and the durability is poor; since the adsorption amount of polyphenols with antioxidant effect is reduced, the yellowing resistance is poor.
[0111] Comparative Example 2
[0112] A method for preparing a durable antistatic polyester fabric is basically the same as that of Example 6, except that catechin is not added in step (3).
[0113] Before soap washing, the peak voltage of the durable antistatic polyester fabric was 800 V, the electrostatic half-life was 110 s, and the moisture regain was 0.45±0.04%; after 5 soap washings, the peak voltage of the durable antistatic polyester fabric was 880 V, the electrostatic half-life was 121 s, and the moisture regain was 0.42±0.02%; the whiteness of the durable antistatic polyester fabric was 77%.
[0114] Comparing Comparative Example 2 with Example 6, it can be found that the peak voltage and electrostatic half-life of Comparative Example 2 are increased, and the whiteness is reduced. This is because catechins are biomass polyphenols, which can bind water molecules on the surface of PET fibers through hydrogen bonds, providing hydrophilic and antistatic functions; in addition, catechins are natural polyphenols, which mainly play an antioxidant role and have the function of reducing the production of unsaturated acids to reduce yellowing. Therefore, Comparative Example 2 without catechins has high peak voltage and electrostatic half-life, and low whiteness.
[0115] Comparative Example 3
[0116] A method for preparing a durable antistatic polyester fabric is basically the same as that of Example 6, except that caffeic acid is not added in step (3).
[0117] Before soap washing, the peak voltage of the durable antistatic polyester fabric was 834 V, the electrostatic half-life was 122 s, and the moisture regain was 0.43±0.04%; after 5 soap washings, the peak voltage of the durable antistatic polyester fabric was 890 V, the electrostatic half-life was 128 s, and the moisture regain was 0.41±0.02%.
[0118] By comparing Comparative Example 3 with Example 6, it can be found that the peak voltage and electrostatic half-life of Comparative Example 3 are high. This is because caffeic acid provides acidic conditions for the dissolution of chitosan. Comparative Example 3 does not add caffeic acid, the acidity is weak, and the solubility of chitosan is reduced, resulting in a decrease in cross-linking efficiency during baking, affecting the antistatic performance.
[0119] Comparative Example 4
[0120] A method for preparing a durable antistatic polyester fabric is basically the same as that of Example 6, except that tea saponin is not added in step (3).
[0121] Before soap washing, the peak voltage of the durable antistatic polyester fabric was 444V, and the static half-life was 68s. After 5 soap washings, the peak voltage of the durable antistatic polyester fabric was 720V, and the static half-life was 84s.
[0122] By comparing Comparative Example 4 with Example 6, it can be found that the peak voltage and electrostatic half-life of Comparative Example 4 are increased. This is because tea saponin plays a role in stabilizing the dispersion of ink and promoting penetration. Without tea saponin, the antistatic performance will decrease.
[0123] Comparative Example 5
[0124] A method for preparing a durable antistatic polyester fabric is basically the same as that of Example 6, except that in step (3), sodium phytate is replaced by sodium hypophosphite.
[0125] Before soap washing, the peak voltage of the durable antistatic polyester fabric was 365V and the static half-life was 65s; after 5 soap washings, the peak voltage of the durable antistatic polyester fabric was 575V and the static half-life was 77s.
[0126] By comparing Comparative Example 5 with Example 6, it can be found that the peak voltage and electrostatic half-life of Comparative Example 5 are increased. This is because sodium hypophosphite is an inorganic salt, which is suitable for hydrophilic cellulose and can penetrate into the interior, but is not as affinity for hydrophobic PET as organic sodium phytate for PET fibers. The organic sodium phytate is more easily adsorbed on the surface of PET to catalyze the reaction. Therefore, sodium phytate is more suitable for polyester modification than sodium hypophosphite and has a better effect.
Claims
1. A method for preparing a durable antistatic polyester fabric, characterized in that: Firstly, a polyester fabric is subjected to a surface activation treatment, and then the polyester fabric after the surface activation treatment is impregnated with a hydroxypropyl trimethyl ammonium chloride chitosan solution, and then a reactive biomass antistatic ink is used to spray the polyester fabric impregnated with the hydroxypropyl trimethyl ammonium chloride chitosan solution, and then a catalytic cross-linking reaction is carried out under a baking condition, and finally the polyester fabric after the reaction is subjected to a plasma treatment to obtain a durable antistatic polyester fabric; The method for surface activation treatment of polyester fabric is as follows: placing the polyester fabric in a natural eutectic solvent and treating it at a temperature of 60-80°C for 30-60 minutes; The natural eutectic solvent is composed of a hydrogen bond donor and a hydrogen bond acceptor, and the molar ratio of the hydrogen bond donor to the hydrogen bond acceptor is 0.5~4:1; The hydrogen bond donor is D-glucose, D-fructose, citric acid, L-malic acid, xylitol or menthol, and the hydrogen bond acceptor is choline chloride, betaine or proline; The preparation process of the reactive biomass antistatic ink is as follows: chitosan, catechin, caffeic acid, tea saponin, citric acid, butane tetracarboxylic acid and sodium phytate are mixed and dissolved in water, first stirred at 800 rpm in a magnetic stirrer for 20 minutes, and then treated in an ultrasonic processor at a power of 100-500 W for 5-20 minutes; The mass ratio of chitosan, catechin, caffeic acid, tea saponin, citric acid, butane tetracarboxylic acid and sodium phytate is 1:2~6:2~6:4~5:6~10:6~10:8~10; the total concentration of the reactive biomass antistatic ink is 20~50g / L; The atmosphere of plasma treatment is oxygen, the power is 5~30W, and the time is 1~3min.
2. The method for preparing a durable antistatic polyester fabric according to claim 1, characterized in that: The mass volume ratio of polyester fabric to natural eutectic solvent is 1 g:100 mL.
3. The method for preparing a durable antistatic polyester fabric according to claim 1, characterized in that: The concentration of the hydroxypropyl trimethyl ammonium chloride chitosan solution is 1-5 g / L; the rolling rate of the polyester fabric after surface activation treatment is 50-80% after being dipped in the hydroxypropyl trimethyl ammonium chloride chitosan solution.
4. The method for preparing a durable antistatic polyester fabric according to claim 1, characterized in that: The baking conditions are: pre-baking at 80°C for 60 minutes, and then baking at 100~140°C for 2~15 minutes.
5. The method for preparing a durable antistatic polyester fabric according to claim 1, characterized in that: When not washed with soap, the peak voltage of durable antistatic polyester fabric is 52~250V, and the static half-life is 0.2~43s; Compared with the case without soap washing, after 5 soap washings, the peak voltage of the durable antistatic polyester fabric changes by no more than 8%, and the static half-life changes by no more than 20%; Compared with the case without soap washing, after 20 soap washings, the peak voltage of the durable antistatic polyester fabric changes by no more than 15%, and the static half-life changes by no more than 30%.
6. The method for preparing a durable antistatic polyester fabric according to claim 1, characterized in that: The whiteness of durable antistatic polyester fabric is not less than 78%.
Citation Information
Patent Citations
Choline chloride based green solvents for polyester dyeing
IN201721018667A
Substituted hydrocarbyl functional siloxanes for household, health, and personal care applications
US20030228333A1
Cited By
Skin-friendly antibacterial polyester blended fabric and preparation method thereof
CN122428516A