A method for preparing 6N grade rhenium powder
Through γ-MnO2 oxidation adsorption and flocculation treatment combined with cation exchange, 6N grade rhenium powder was successfully prepared, which solved the problem of insufficient purity of rhenium powder in the existing technology and achieved efficient rhenium powder preparation and industrial production.
Patent Information
- Application Number
- CN202410955750.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-17
AI Technical Summary
It is difficult to prepare ultra-high purity rhenium powder of more than 99.9999% 6N grade with existing technology, and there are few methods in industrial production that can effectively remove metal impurities in ammonium rhenate, resulting in insufficient purity of rhenium powder.
The oxidative adsorption and flocculation treatment of γ-MnO2 is combined with a cation exchange resin, and through multiple impurity removal treatments, high-purity ammonium rhenate is prepared, and reduction roasting is performed in a hydrogen atmosphere to obtain 6N grade rhenium powder.
It achieves high-purity preparation of rhenium powder, avoids the complexity of recrystallization and purification, has the characteristics of energy saving, simple operation, and is easy for industrial process production.
Smart Images

Figure CN118492384B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of rhenium powder preparation, and in particular to a method for preparing 6N grade rhenium powder. Background Art
[0002] Rhenium metal has a melting point of 3180℃, second only to tungsten at 3410℃, and is a refractory metal. Rhenium is rare and dispersed in the earth's crust, and is one of the rarest elements in the earth's crust. Its average content is estimated to be one billionth, making it a rare metal. Rhenium has developed into an important strategic resource. In recent years, with the development of the electronics industry and semiconductor materials, there has been a demand for 6N grade ultra-high purity rhenium of more than 99.9999%.
[0003] Rhenium has no independent deposits and mainly comes from byproducts of copper and molybdenum smelting processes. Rhenium is mainly produced by highly purifying ammonium rhenate raw materials through extraction, ion exchange and recrystallization, and then reducing them with hydrogen. However, most of the existing industrial methods are above 99.99%, and there are few methods for preparing 6N ultra-high purity rhenium above 99.9999%. Summary of the invention
[0004] The purpose of this application is to provide a method for preparing 6N grade rhenium powder to solve the above problems.
[0005] To achieve the above objectives, the present application provides a method for preparing 6N grade rhenium powder, comprising:
[0006] ammonium rhenate, high-purity water and activated carbon are mixed and filtered to obtain a first ammonium rhenate solution;
[0007] The first ammonium rhenate solution and γ-MnO2 are mixed and stirred to obtain a second ammonium rhenate solution;
[0008] The second ammonium rhenate solution and the flocculant are mixed, stirred for a second time, and allowed to stand to obtain a third ammonium rhenate solution;
[0009] Filtering the third ammonium rhenate solution to obtain a fourth ammonium rhenate solution;
[0010] The fourth ammonium rhenate solution is treated with a cationic resin to obtain a fifth ammonium rhenate solution;
[0011] The fifth ammonium rhenate solution is heated and evaporated to obtain an ammonium rhenate concentrate, the ammonium rhenate concentrate is mixed with electronic grade ammonia water to obtain a sixth ammonium rhenate solution, the sixth ammonium rhenate solution is frozen and crystallized, and dried to obtain ammonium rhenate crystals;
[0012] Under a hydrogen atmosphere, the ammonium rhenate crystals are reduction-calcined to obtain the 6N grade rhenium powder.
[0013] Optionally, the preparation method of the 6N grade rhenium powder satisfies at least one of the following conditions:
[0014] A. The purity of the ammonium rhenate is 99%-99.9%;
[0015] B. The mass ratio of the ammonium rhenate to the high-purity water is 1:(18-25).
[0016] Optionally, the preparation method of the 6N grade rhenium powder satisfies at least one of the following conditions:
[0017] A. The mass ratio of the γ-MnO2 to the ammonium rhenate is (0.2%-2%): 1;
[0018] B. The first stirring time is 30 min-60 min, and the speed is 100 r / min-300 r / min.
[0019] Optionally, the preparation method of the 6N grade rhenium powder satisfies at least one of the following conditions:
[0020] A. The mass ratio of the flocculant to the γ-MnO2 is (1%-10%): 1;
[0021] B. The second stirring time is 10min-30min, and the speed is 100r / min-300r / min;
[0022] C. The standing time is 30min-120min;
[0023] D. The flocculant includes polyacrylamide flocculant.
[0024] Optionally, the filtration includes a first filtration and a second filtration, and the preparation method of the 6N grade rhenium powder satisfies at least one of the following conditions:
[0025] A. The applied pressure of the first filtration is 0.1Mpa-0.2Mpa;
[0026] B. The pore size of the filter membrane used for the first filtration is 50 μm-100 μm.
[0027] Optionally, the preparation method of the 6N grade rhenium powder satisfies at least one of the following conditions:
[0028] A. The second filtration adopts step-by-step filtration, and the pore size distribution of the filter membrane of the step-by-step filtration is 1μm-3μm, 0.4μm-0.9μm and 0.1μm-0.3μm;
[0029] B. The applied pressure of the second filtration is 0.05Mpa-0.1Mpa.
[0030] Optionally, the cationic resin comprises a hydrogen-type cationic resin.
[0031] Optionally, the preparation method of the 6N grade rhenium powder satisfies at least one of the following conditions:
[0032] A. the pH of the sixth ammonium rhenate solution is 8-10;
[0033] B. The volume of the ammonium rhenate concentrate is 20%-30% of the fifth ammonium rhenate solution.
[0034] Optionally, the ammonium rhenate crystals are sieved before the reduction roasting, and the mesh size of the sieve is 40-80.
[0035] Optionally, the reduction roasting includes a first reduction roasting and a second reduction roasting, and the preparation method of the 6N grade rhenium powder satisfies at least one of the following conditions:
[0036] A. The temperature of the first reduction roasting is 300°C-350°C, and the time is 4h-6h;
[0037] B. The temperature of the second reduction roasting is 650°C-750°C, and the time is 4h-6h.
[0038] Compared with the prior art, the beneficial effects of this application include:
[0039] The preparation method of 6N grade rhenium powder provided in the present application uses γ-MnO2 with super strong oxidizing and adsorbing properties to fully oxidize the cations in ammonium rhenate into a high-valent state and adsorb them. The metal impurity ions in the ammonium rhenate undergo a hydrolysis reaction to form hydroxyl cations. These hydroxyl cations can react with γ-MnO2 to form inner circle complexes with stable properties, and then specific adsorption occurs. In this specific adsorption process, Mn 2+ and H + The metal impurity ions form a stable complex in the inner ring of the γ-MnO2 structure, while the Mn 2+ The ion exchange occurs with the metal impurity ions, or the hydroxyl groups on its surface react with the metal impurity ions to form hydroxyl complexes. After the γ-MnO2 is adsorbed, the added manganese dioxide and impurities are removed by flocculation and two-stage filtration. In view of the high cation concentration in the ammonium rhenate solution, cation exchange is used to achieve the NH4 + The batch removal of ions and the deep removal of other impurity ions realize the preparation of 6N grade ammonium rhenate; the present application obtains extremely high-purity 6N ammonium rhenate through multiple impurity removal treatments such as activated carbon adsorption, γ-MnO2 oxidation adsorption, two-stage filtration separation and ion exchange removal. This method is easy to realize process-based industrial preparation, avoids the purification method of multiple recrystallization of ammonium rhenate, and has the characteristics of energy saving and simple operation. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0041] Figure 1 This is a scanning electron microscope image of the 6N grade rhenium powder prepared in Example 1;
[0042] Figure 2 This is a scanning electron microscope image of the rhenium powder prepared in Comparative Example 11. DETAILED DESCRIPTION
[0043] As used herein:
[0044] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0045] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0046] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0047] In these examples, parts and percentages are by mass unless otherwise indicated.
[0048] "Mass parts" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass parts of component A are a parts and the mass parts of component B are b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass parts of all components is not limited to 100 parts.
[0049] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0050] The present application adopts a strong oxidation adsorption removal method combined with ion exchange and membrane separation to treat 99% low-purity ammonium rhenate, and controls the environment of the subsequent reduction process to prepare 6N purity rhenium powder.
[0051] The present application provides a method for preparing 6N grade rhenium powder, comprising:
[0052] ammonium rhenate, high-purity water and activated carbon are mixed and filtered to obtain a first ammonium rhenate solution;
[0053] The first ammonium rhenate solution and γ-MnO2 are mixed and stirred to obtain a second ammonium rhenate solution;
[0054] The second ammonium rhenate solution and the flocculant are mixed, stirred for a second time, and allowed to stand to obtain a third ammonium rhenate solution;
[0055] Filtering the third ammonium rhenate solution to obtain a fourth ammonium rhenate solution;
[0056] The fourth ammonium rhenate solution is treated with a cationic resin to obtain a fifth ammonium rhenate solution;
[0057] The fifth ammonium rhenate solution is heated and evaporated to obtain an ammonium rhenate concentrate, the ammonium rhenate concentrate is mixed with electronic grade ammonia water to obtain a sixth ammonium rhenate solution, the sixth ammonium rhenate solution is frozen and crystallized, and dried to obtain ammonium rhenate crystals;
[0058] Under a hydrogen atmosphere, the ammonium rhenate crystals are reduction-calcined to obtain the 6N grade rhenium powder.
[0059] It should be noted that MnO2 has many variants, such as α-MnO2, β-MnO2, γ-MnO2, δ-MnO2, etc. In fact, γ-MnO2 has the strongest oxidation and adsorption capabilities, and can simultaneously oxidize the cations in the ammonium rhenate solution to a high valence state and adsorb them, thereby achieving an impurity removal effect; γ-MnO2 is composed of octahedral units of manganese and oxygen atoms, forming irregular alternating growth of pyrolusite [1×1] tunnels and rhombus-type [1×2] tunnel units in one-dimensional direction. This disordered alternating growth structure leads to the formation of a large number of defects, vacancies and non-ideal ratios in the crystal. Vacancies play an important role in the chemical adsorption properties of Mn(IV) oxide.
[0060] In some embodiments, the method for preparing the 6N grade rhenium powder satisfies at least one of the following conditions:
[0061] A. The purity of the ammonium rhenate is 99%-99.9%;
[0062] Optionally, the purity of ammonium rhenate may be 99%, 99.1%, 99.2%, 99.3%, 99.4%, 99.5%, 99.6%, 99.7%, 99.8%, 99.9%, or any value between 99% and 99.9%;
[0063] B. The mass ratio of the ammonium rhenate to the high-purity water is 1:(18-25).
[0064] Optionally, the mass ratio of ammonium rhenate to high-purity water can be 1:18, 1:19, 1:20, 1:21, 1:22, 1:23, 1:24, 1:25 or any value between 1:(18-25).
[0065] In some embodiments, the method for preparing the 6N grade rhenium powder satisfies at least one of the following conditions:
[0066] A. The mass ratio of the γ-MnO2 to the ammonium rhenate is (0.2%-2%): 1;
[0067] Optionally, the mass ratio of γ-MnO2 to ammonium rhenate can be 0.2%:1, 0.4%:1, 0.6%:1, 0.8%:1, 1%:1, 1.2%:1, 1.4%:1, 1.6%:1, 1.8%:1, 2%:1 or any value between (0.2%-2%):1;
[0068] It should be noted that the mass ratio of γ-MnO2 to ammonium rhenate is (0.2%-2%): 1. When the usage of γ-MnO2 is less than 0.2%, the oxidation capacity is insufficient, and the oxidation and adsorption effects are not good; when the usage of γ-MnO2 is higher than 2%, the oxidation and adsorption capacity is excessive, and more auxiliary materials need to be added in the subsequent flocculation and filtration steps.
[0069] B. The first stirring time is 30 min-60 min, and the speed is 100 r / min-300 r / min.
[0070] Optionally, the first stirring time can be 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min or any value between 30 min and 60 min, and the speed can be 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min or any value between 100 r / min and 300 r / min.
[0071] In some embodiments, the method for preparing the 6N grade rhenium powder satisfies at least one of the following conditions:
[0072] A. The mass ratio of the flocculant to the γ-MnO2 is (1%-10%): 1;
[0073] Optionally, the mass ratio of the flocculant to γ-MnO2 can be 1%:1, 2%:1, 3%:1, 4%:1, 5%:1, 6%:1, 7%:1, 8%:1, 9%:1, 10%:1 or any value between (1%-10%):1;
[0074] It should be noted that when the mass ratio of flocculant to γ-MnO2 is less than 1%:1, the flocculant content in the solution is small, the dispersion is uneven, and the co-precipitation effect with the solid impurity particles is poor. When the mass ratio of flocculant to γ-MnO2 is higher than 10%:1, it is easy to cause excessive flocculant to form gel in local areas of the solution, affecting the overall co-precipitation effect of the solution.
[0075] B. The second stirring time is 10min-30min, and the speed is 100r / min-300r / min;
[0076] Optionally, the second stirring time can be 10 min, 15 min, 20 min, 25 min, 30 min or any value between 10 min and 30 min, and the speed can be 100 r / min, 150 r / min, 200 r / min, 250 r / min, 300 r / min or any value between 100 r / min and 300 r / min.
[0077] C. The standing time is 30min-120min;
[0078] Optionally, the standing time can be 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min or any value between 30 min and 120 min;
[0079] D. The flocculant includes polyacrylamide flocculant.
[0080] It should be noted that since the γ-MnO2 particles after adsorption show electrical repulsion and dispersion, they have no coagulation effect, and the direct filtration effect is poor at this time. The performance of polyacrylamide flocculant is reflected in the formation of polymers with discrete γ-MnO2 in the solution, and the added γ-MnO2 particles are brought close to each other. By using polyacrylamide flocculant to enrich the γ-MnO2 particles, the polyacrylamide flocculant with negatively charged groups and the positively charged γ-MnO2 particles can be accelerated to approach each other. Its polymerization properties make these particles concentrated and form polymer precipitates, which are easy to remove.
[0081] In some embodiments, the filtration includes a first filtration and a second filtration, and the preparation method of the 6N grade rhenium powder satisfies at least one of the following conditions:
[0082] A. The applied pressure of the first filtration is 0.1Mpa-0.2Mpa;
[0083] Optionally, the applied pressure of the first filtration may be 0.1 MPa, 0.11 MPa, 0.12 MPa, 0.13 MPa, 0.14 MPa, 0.15 MPa, 0.16 MPa, 0.17 MPa, 0.18 MPa, 0.19 MPa, 0.2 MPa or any value between 0.1 MPa and 0.2 MPa;
[0084] B. The pore size of the filter membrane used for the first filtration is 50 μm-100 μm.
[0085] Optionally, the pore size of the filter membrane for the first filtration may be 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm or any value between 50 μm and 100 μm.
[0086] In some embodiments, the method for preparing the 6N grade rhenium powder satisfies at least one of the following conditions:
[0087] A. The second filtration adopts step-by-step filtration, and the pore size distribution of the filter membrane of the step-by-step filtration is 1μm-3μm, 0.4μm-0.9μm and 0.1μm-0.3μm;
[0088] Optionally, while ensuring the stability of the filter membrane pore size, precise filtration of impurities of different particle sizes is achieved, and step-by-step filtration is adopted, and filter membranes with pore sizes of 1μm-3μm, 0.4μm-0.9μm and 0.1μm-0.3μm are sequentially passed through, firstly, 1μm, 1.5μm, 2μm, 2.5μm, 3μm or any value between 1μm-3μm can be passed, secondly, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm or any value between 0.4μm-0.9μm can be passed, and finally, 0.1μm, 0.15μm, 0.2μm, 0.25μm, and any value between 0.3μm can be passed;
[0089] B. The applied pressure of the second filtration is 0.05Mpa-0.1Mpa.
[0090] Optionally, the applied pressure of the second filtration may be 0.05 MPa, 0.06 MPa, 0.07 MPa, 0.08 MPa, 0.09 MPa, 0.1 MPa or any value between 0.05 MPa and 0.1 MPa.
[0091] It should be noted that first, a large number of γ-MnO2 aggregate particles are quickly intercepted by large-pore filter paper (pore size is 50μm-100μm), and then 1μm-3μm, 0.4μm-0.9μm and 0.1μm-0.3μm microporous filter membranes are used step by step; γ-MnO2 oxidizes and adsorbs impurity ions and combines well with flocculants to form aggregate particles. After step-by-step filtration, the solid γ-MnO2 particles that adsorb a large number of cationic impurities can be completely removed, thereby achieving rapid adsorption and removal of a large number of impurities in ammonium rhenate and quickly improving the purity of ammonium rhenate.
[0092] It should also be noted that the remaining larger particles of γ-MnO2 flocculation products in the third ammonium rhenate solution are removed by relatively increased pressure, and then the smaller-sized solid impurity particles are precisely filtered and removed by relatively small pressure, and the fourth ammonium rhenate solution after the second impurity removal is obtained by different graded filter membranes.
[0093] In some embodiments, the cationic resin comprises a hydrogen-form cationic resin.
[0094] It should be noted that after γ-MnO2 oxidizes and adsorbs impurity ions in the ammonium rhenate solution, the number of positively charged cationic impurities in the solution is small. Hydrogen-type cationic resin is selected to achieve deep removal of the remaining trace amounts of other impurity ions without introducing other impurities.
[0095] In some embodiments, the method for preparing the 6N grade rhenium powder satisfies at least one of the following conditions:
[0096] A. the pH of the sixth ammonium rhenate solution is 8-10;
[0097] Optionally, the pH of the sixth ammonium rhenate solution may be 8, 8.5, 9, 9.5, 10 or any value between 8 and 10;
[0098] B. The volume of the ammonium rhenate concentrate is 20%-30% of the fifth ammonium rhenate solution.
[0099] Optionally, the volume of the ammonium rhenate concentrate can be 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30% or any value between 20% and 30% of the fifth ammonium rhenate solution.
[0100] In some embodiments, the ammonium rhenate crystals are sieved before the reduction roasting, and the mesh size of the sieve is 40-80.
[0101] Optionally, the mesh size of the sieve can be 40, 45, 50, 55, 60, 65, 70, 75, 80 or any value between 40 and 80.
[0102] In some embodiments, the reduction roasting includes a first reduction roasting and a second reduction roasting, and the preparation method of the 6N grade rhenium powder satisfies at least one of the following conditions:
[0103] A. The temperature of the first reduction roasting is 300°C-350°C, and the time is 4h-6h;
[0104] Optionally, the temperature of the first reduction roasting may be 300°C, 305°C, 310°C, 315°C, 320°C, 325°C, 330°C, 335°C, 340°C, 345°C, 350°C or any value between 300°C and 350°C, and the time may be 4h, 4.5h, 5h, 5.5h, 6h or any value between 4h and 6h;
[0105] B. The temperature of the second reduction roasting is 650°C-750°C, and the time is 4h-6h.
[0106] Optionally, the temperature of the second reduction roasting can be 650℃, 660℃, 670℃, 680℃, 690℃, 700℃, 710℃, 720℃, 730℃, 740℃, 750℃ or any value between 650℃-750℃, and the time can be 4h, 4.5h, 5h, 5.5h, 6h or any value between 4h-6h.
[0107] It should be noted that the two-step reduction roasting can prevent the grain growth of rhenium powder and obtain high-quality rhenium powder. At the same time, the lower secondary reduction temperature of 650℃-750℃ avoids the volatilization contamination of impurities in the high-temperature furnace tube during higher temperature reduction, which reduces the purity of the rhenium powder.
[0108] It should also be noted that during the reduction roasting process, the boats and furnace tubes used in the operation process can be coated with rhenium to avoid contamination, and the screen material is a non-metallic nylon screen.
[0109] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0110] Example 1
[0111] This embodiment provides a method for preparing 6N grade rhenium powder, which specifically includes:
[0112] S1: dissolving ammonium rhenate with a purity of 99% in high-purity water at room temperature, wherein the mass ratio of ammonium rhenate to high-purity water is 1:20, removing solid impurities in the ammonium rhenate solution by adsorbing activated carbon, and filtering to obtain a first ammonium rhenate solution after the first impurity removal;
[0113] S2: adding γ-MnO2 to the first ammonium rhenate solution, wherein the amount of γ-MnO2 added is 0.2% of the mass of the ammonium rhenate, and stirring for 30 minutes to obtain a second ammonium rhenate solution;
[0114] S3: adding polyacrylamide flocculant to the second ammonium rhenate solution, the mass ratio of polyacrylamide added to γ-MnO2 being 1%:1, stirring for 10 minutes, standing for 30 minutes, and obtaining a layered third ammonium rhenate solution;
[0115] S4: performing a first filtration and a second filtration on the third ammonium rhenate solution in sequence, wherein the first filtration applies a pressure of 0.1 MPa to pass through a filter membrane with a pore size of 50 μm, and the second filtration applies a pressure of 0.05 MPa to pass through filter membranes with pore sizes of 1 μm, 0.45 μm, and 0.22 μm in sequence, to obtain a fourth ammonium rhenate solution after the second impurity removal;
[0116] S5: pumping the fourth ammonium rhenate solution into a two-stage hydrogen-type cation exchange resin to obtain a fifth ammonium rhenate solution after the third impurity removal after treatment;
[0117] S6: heating and evaporating the fifth ammonium rhenate solution to 20% of the volume of the original solution to obtain an ammonium rhenate concentrate, adding electronic grade ammonia water to the ammonium rhenate concentrate until the pH value is 8 to obtain a sixth ammonium rhenate solution, freezing the sixth ammonium rhenate solution to -8°C, crushing, drying, and passing through a 40-mesh sieve to obtain ammonium rhenate crystals;
[0118] S7: Under a hydrogen atmosphere, the ammonium rhenate crystals are subjected to a first reduction roasting and a second reduction roasting, wherein the first reduction roasting is carried out at a temperature of 300° C. for 4 hours, and the second reduction roasting is carried out at a temperature of 650° C. for 4 hours, to obtain 6N grade rhenium powder.
[0119] The scanning electron microscope image of the 6N grade rhenium powder is as follows Figure 1 shown.
[0120] Example 2
[0121] This embodiment provides a method for preparing 6N grade rhenium powder, which specifically includes:
[0122] S1: dissolving ammonium rhenate with a purity of 99% in high-purity water at room temperature, wherein the mass ratio of ammonium rhenate to high-purity water is 1:20, removing solid impurities in the ammonium rhenate solution by adsorbing activated carbon, and filtering to obtain a first ammonium rhenate solution after the first impurity removal;
[0123] S2: adding γ-MnO2 to the first ammonium rhenate solution, wherein the amount of γ-MnO2 added is 1.0% of the mass of the ammonium rhenate, and stirring for 45 minutes to obtain a second ammonium rhenate solution;
[0124] S3: adding polyacrylamide flocculant to the second ammonium rhenate solution, the mass ratio of polyacrylamide added to γ-MnO2 being 5%:1, stirring for 20 minutes, standing for 60 minutes, and obtaining a layered third ammonium rhenate solution;
[0125] S4: performing a first filtration and a second filtration on the third ammonium rhenate solution in sequence, wherein the first filtration applies a pressure of 0.15 MPa to pass through a filter membrane with a pore size of 80 μm, and the second filtration applies a pressure of 0.08 MPa to pass through filter membranes with pore sizes of 1 μm, 0.45 μm, and 0.22 μm in sequence, to obtain a fourth ammonium rhenate solution after the second impurity removal;
[0126] S5: pumping the fourth ammonium rhenate solution into a two-stage hydrogen-type cation exchange resin to obtain a fifth ammonium rhenate solution after the third impurity removal after treatment;
[0127] S6: heating and evaporating the fifth ammonium rhenate solution to 25% of the volume of the original solution to obtain an ammonium rhenate concentrate, adding electronic grade ammonia water to the ammonium rhenate concentrate until the pH value is 9 to obtain a sixth ammonium rhenate solution, freezing the sixth ammonium rhenate solution to -12°C, crushing, drying, and passing through a 40-mesh sieve to obtain ammonium rhenate crystals;
[0128] S7: Under a hydrogen atmosphere, the ammonium rhenate crystals are subjected to a first reduction roasting and a second reduction roasting, wherein the first reduction roasting is carried out at a temperature of 320° C. for 5 hours, and the second reduction roasting is carried out at a temperature of 700° C. for 5 hours, to obtain 6N grade rhenium powder.
[0129] Example 3
[0130] This embodiment provides a method for preparing 6N grade rhenium powder, which specifically includes:
[0131] S1: dissolving ammonium rhenate with a purity of 99% in high-purity water at room temperature, wherein the mass ratio of ammonium rhenate to high-purity water is 1:20, removing solid impurities in the ammonium rhenate solution by adsorbing activated carbon, and filtering to obtain a first ammonium rhenate solution after the first impurity removal;
[0132] S2: adding γ-MnO2 to the first ammonium rhenate solution, wherein the amount of γ-MnO2 added is 2% of the mass of the ammonium rhenate, and stirring for 60 minutes to obtain a second ammonium rhenate solution;
[0133] S3: adding polyacrylamide flocculant to the second ammonium rhenate solution, the mass ratio of polyacrylamide added to γ-MnO2 being 10%:1, stirring for 30 minutes, standing for 120 minutes, and obtaining a layered third ammonium rhenate solution;
[0134] S4: performing a first filtration and a second filtration on the third ammonium rhenate solution in sequence, wherein the first filtration applies a pressure of 0.2 MPa to pass through a filter membrane with a pore size of 100 μm, and the second filtration applies a pressure of 0.1 MPa to pass through filter membranes with pore sizes of 1 μm, 0.45 μm, and 0.22 μm in sequence, to obtain a fourth ammonium rhenate solution after the second impurity removal;
[0135] S5: pumping the fourth ammonium rhenate solution into a two-stage hydrogen-type cation exchange resin to obtain a fifth ammonium rhenate solution after the third impurity removal after treatment;
[0136] S6: heating and evaporating the fifth ammonium rhenate solution to 30% of the volume of the original solution to obtain an ammonium rhenate concentrate, adding electronic grade ammonia water to the ammonium rhenate concentrate until the pH value is 10 to obtain a sixth ammonium rhenate solution, freezing the sixth ammonium rhenate solution to -18°C, crushing, drying, and passing through a 40-mesh sieve to obtain ammonium rhenate crystals;
[0137] S7: Under a hydrogen atmosphere, the ammonium rhenate crystals are subjected to a first reduction roasting and a second reduction roasting, wherein the first reduction roasting is carried out at a temperature of 350° C. for 6 hours, and the second reduction roasting is carried out at a temperature of 750° C. for 6 hours, to obtain 6N grade rhenium powder.
[0138] Comparative Example 1
[0139] This comparative example provides a method for preparing rhenium powder, which is different from Example 1 in that the MnO2 in this comparative example is α-MnO2, and the other conditions are consistent with Example 1.
[0140] Comparative Example 2
[0141] This comparative example provides a method for preparing rhenium powder, which is different from Example 1 in that the MnO2 in this comparative example is β-MnO2, and the other conditions are consistent with Example 1.
[0142] Comparative Example 3
[0143] This comparative example provides a method for preparing rhenium powder, which is different from Example 1 in that the MnO2 in this comparative example is δ-MnO2, and the other conditions are consistent with Example 1.
[0144] Comparative Example 4
[0145] This comparative example provides a method for preparing rhenium powder, which is different from Example 1 in that MnO2 is not added in this comparative example, and the other conditions are the same as those in Example 1.
[0146] Comparative Example 5
[0147] This comparative example provides a method for preparing rhenium powder, which is different from Example 1 in that no flocculant is added in this comparative example, and the other conditions are the same as those in Example 1.
[0148] Comparative Example 6
[0149] This comparative example provides a method for preparing rhenium powder, which is different from Example 1 in that the flocculant added in this comparative example is polyaluminum chloride, and the other conditions are the same as those in Example 1.
[0150] Comparative Example 7
[0151] This comparative example provides a method for preparing rhenium powder, which is different from Example 1 in that the mass ratio of the flocculant added in this comparative example to γ-MnO2 is 20%:1, and the other conditions are consistent with Example 1.
[0152] Comparative Example 8
[0153] This comparative example provides a method for preparing rhenium powder, which is different from Example 1 in that only one filtration is performed in this comparative example, and a pressure of 0.1 MPa is applied to pass through a filter membrane with a pore size of 50 μm, and the other conditions are consistent with Example 1.
[0154] Comparative Example 9
[0155] This comparative example provides a method for preparing rhenium powder, which is different from Example 1 in that: this comparative example performs a first filtration and a second filtration, wherein the first filtration applies a pressure of 0.05 MPa to pass through a filter membrane with a pore size of 200 μm, and the second filtration applies a pressure of 0.02 MPa to pass through filter membranes with pore sizes of 8 μm, 3.0 μm and 0.8 μm in sequence to obtain a fourth ammonium rhenate solution after the second impurity removal; the other conditions are the same as those in Example 1.
[0156] Comparative Example 10
[0157] This comparative example provides a method for preparing rhenium powder, which is different from Example 1 in that this comparative example does not use cationic resin for treatment, and the other conditions are consistent with Example 1.
[0158] Comparative Example 11
[0159] This comparative example provides a method for preparing rhenium powder, which is different from Example 1 in that only one reduction roasting is performed in this comparative example, the temperature of the reduction roasting is 700° C., the time is 6 h, and the other conditions are consistent with Example 1.
[0160] The scanning electron microscope image of the rhenium powder is as follows Figure 2 shown.
[0161] Based on the settings of the above embodiments and comparative examples, the obtained rhenium powder was tested for purity, and the test results are shown in Table 1;
[0162] Table 1 Purity test
[0163]
[0164] Purity detection: The purity of rhenium powder is detected by glow discharge mass spectrometry, which is an analytical method that uses a glow discharge source as an ion source and connects it to a mass spectrometer for mass spectrometry. Glow discharge mass spectrometry is a common method for analyzing impurity components of high-purity materials. Glow discharge mass spectrometry is used to determine the content of various impurity elements in rhenium powder and calculate the sum value, which is recorded as (1-the sum value of impurity elements) × 100% as the element purity.
[0165] It can be seen from the above embodiments and comparative examples that the added oxidant is manganese dioxide other than γ-MnO2, and the purity can only reach 5N but cannot reach 6N; the purity is only 4N if no oxidant is added; no flocculant is added or other flocculants are added, resulting in incomplete removal of impurities and a purity of 4N; the flocculant content is too high and the purity cannot reach 5N; only application and filtration or the filtration membrane size is not within the range, the purity can only reach 4N; however, the purity of the cationic resin is 4N; the purity is 6N after only one calcination, but the powder particle size is coarse.
[0166] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0167] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for preparing 6N grade rhenium powder, characterized in that: include: ammonium rhenate, high-purity water and activated carbon are mixed and filtered to obtain a first ammonium rhenate solution; Mixing the first ammonium rhenate solution and γ-MnO2 and stirring for a first time to obtain a second ammonium rhenate solution; The second ammonium rhenate solution and the flocculant are mixed, stirred for a second time, and allowed to stand to obtain a third ammonium rhenate solution; filtering the third ammonium rhenate solution to obtain a fourth ammonium rhenate solution; The fourth ammonium rhenate solution is treated with a cationic resin to obtain a fifth ammonium rhenate solution; The fifth ammonium rhenate solution is heated and evaporated to obtain an ammonium rhenate concentrate, the ammonium rhenate concentrate is mixed with electronic grade ammonia water to obtain a sixth ammonium rhenate solution, the sixth ammonium rhenate solution is freeze-crystallized, and dried to obtain ammonium rhenate crystals; Under a hydrogen atmosphere, the ammonium rhenate crystals are subjected to reduction roasting to obtain the 6N grade rhenium powder; The mass ratio of the γ-MnO2 to the ammonium rhenate is (0.2%-2%): 1; The flocculant includes a polyacrylamide flocculant; The cationic resin includes a hydrogen-type cationic resin; The filtering includes a first filtering and a second filtering; The applied pressure of the first filtration is 0.1Mpa-0.2Mpa; The pore size of the filter membrane of the first filtration is 50 μm-100 μm; The second filtration adopts step-by-step filtration, and the pore size distribution of the filter membrane of the step-by-step filtration is 1 μm-3 μm, 0.4 μm-0.9 μm and 0.1 μm-0.3 μm; The applied pressure of the second filtration is 0.05Mpa-0.1Mpa; The reduction roasting includes a first reduction roasting and a second reduction roasting; The temperature of the first reduction roasting is 300-350°C, and the time is 4-6 hours; The temperature of the second reduction roasting is 650° C.-750° C., and the time is 4 h-6 h.
2. The method for preparing 6N grade rhenium powder according to claim 1, wherein: At least one of the following conditions is met: A. The purity of the ammonium rhenate is 99%-99.9%; B. The mass ratio of the ammonium rhenate to the high-purity water is 1:(18-25).
3. The method for preparing 6N grade rhenium powder according to claim 1, characterized in that: The first stirring time is 30 min-60 min, and the speed is 100 r / min-300 r / min.
4. The method for preparing 6N grade rhenium powder according to claim 1, characterized in that: At least one of the following conditions is met: A. The mass ratio of the flocculant to the γ-MnO2 is (1%-10%): 1; B. The second stirring time is 10min-30min, and the speed is 100r / min-300r / min; C. The standing time is 30 min-120 min.
5. The method for preparing 6N grade rhenium powder according to claim 1, characterized in that: At least one of the following conditions is met: A. the pH of the sixth ammonium rhenate solution is 8-10; B. The volume of the ammonium rhenate concentrate is 20%-30% of the fifth ammonium rhenate solution.
6. The method for preparing 6N grade rhenium powder according to claim 1, characterized in that: The ammonium rhenate crystals are sieved before the reduction roasting, and the mesh number of the sieve is 40-80.
Citation Information
Patent Citations
Preparation method of superfine rhenium powder
CN101700574A
Preparation method of high purity ammonium rhenate
CN108408785A
Process for the production of ammonium perrhenate
CN109890761A
Rhenium powder and rhenium products with 6N purity and above and preparation method of rhenium powder and rhenium product
CN113333771A
Method for purifying ammonium rhenate
CN114314672A