Preparation method of 2,3,5-trimethylhydroquinone diester
By using modified Fe3O4 particle catalyst and magnetic absorption recovery technology, the equipment corrosion and recovery problems caused by strong acid catalysts in the prior art were solved, and the selectivity and yield of 2,3,5-trimethylhydroquinone diesters were improved. , realizes the recycling of catalysts and efficient utilization of resources.
Patent Information
- Application Number
- CN202410968696.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The prior art uses strong acid catalysts in the synthesis of 2,3,5-trimethylhydroquinone diesters to cause equipment corrosion and difficulty in recycling, and the selectivity and yield are not high.
Using a catalyst system based on hydrophilic Fe3O4 particles, the rearrangement acylation reaction is carried out through sulfonation and composite with mesoporous silica, combined with magnetic absorption and recovery technology, to avoid the use of strong acid catalysts and to continue through the circulation liquid. Use and regulate control by-product concentration.
The selectivity and yield of the reaction are significantly improved, the occurrence of side reactions is reduced, the production cost and environmental burden are reduced, and the catalyst can be recycled through magnetic recycling, improving resource utilization efficiency and product purity.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical synthesis processes, and in particular to a method for preparing 2,3,5-trimethylhydroquinone diester. Background Art
[0002] 2,3,5-Trimethylhydroquinone diester is a chemical that is the esterification product of 2,3,5-trimethylhydroquinone. 2,3,5-Trimethylhydroquinone itself is an important chemical intermediate and is often used in the synthesis of vitamin E. As a derivative, 2,3,5-trimethylhydroquinone diester also has important applications in the chemical and pharmaceutical industries, especially as a key raw material for the synthesis of vitamin E and its acetate. Vitamin E is a fat-soluble vitamin that is essential to human health. It has antioxidant properties, can protect cell membranes from free radical damage, and helps to improve immunity and delay aging. Therefore, 2,3,5-trimethylhydroquinone diester plays a core role in the production of vitamin E-related products, which are widely used in health care products, medicines, cosmetics, and food additives. In addition, due to its special role in the synthesis process, the efficient preparation method of this compound is also one of the hot spots in chemical research and industrial production, such as using bubble tower reactors or ultra-gravity technology to optimize the production process to improve yield and selectivity.
[0003] The prior art method generally comprises the following steps: firstly polymerizing acetone to isophorone, then performing rearrangement oxidation to obtain oxyisophorone, then performing rearrangement acylation to obtain trimethylhydroquinone diacetate, and then performing saponification hydrolysis to obtain trimethylhydroquinone.
[0004]
[0005] The process involves a method for preparing 2,3,5-trimethylhydroquinone diester by aromatizing tea ketone with an acylating agent and an acidic soluble catalyst, and the method can be carried out continuously and intermittently. At the same time, the acylating agent used is carboxylic anhydride, and the conversion rate can be as high as 100%, but the selectivity is only 80%-95%. The main by-product formed is 3,5-diacetoxyacetophenone. In order to separate and purify 2,3,5-trimethylhydroquinone diester after the reaction, it is necessary to add a large amount of water or alkaline aqueous solution to precipitate a mixture of 2,3,5-trimethylhydroquinone diester and 3,5-diacetoxyacetophenone, and purify it by recrystallization from an organic solvent, which will inevitably produce a large amount of wastewater and organic solvents, which will not only lead to the hydrolysis of carboxylic anhydride, but also be accompanied by a large amount of losses, and the strong acid catalyst used may also cause corrosion problems in production equipment, especially for equipment made of non-acid-resistant materials. Long-term operation may cause frequent equipment damage, increase maintenance costs and downtime, so this method has serious defects in terms of economy and environment.
[0006] In general, the isophorone method for synthesizing trimethylhydroquinone has certain advantages. However, in the process of synthesizing 2,3,5-trimethylhydroquinone diester, the strong acid as a catalyst is difficult to recover and causes equipment corrosion. Summary of the invention
[0007] In order to solve the problem that the method for synthesizing 2,3,5-trimethylhydroquinone diester in the prior art is difficult to recycle and corrosive, the present application provides a method for preparing 2,3,5-trimethylhydroquinone diester, the catalyst used in the method has higher selectivity and is easy to recycle, and the by-products in the synthesis continue to accumulate during the circulation process and can also achieve the purpose of recovery.
[0008] The present application provides a method for preparing 2,3,5-trimethylhydroquinone diester, comprising the following steps:
[0009] S1. Adding polyethylene glycol to the aqueous dispersion of hydrophilic Fe3O4 particles under a nitrogen atmosphere, wherein the mass ratio of the hydrophilic Fe3O4 particles to the polyethylene glycol is 0.1-0.2:1, heating and stirring, adding an ammonia solution, continuing stirring, and then centrifuging to collect the lower precipitate, washing to obtain Fe3O4-polyethylene glycol particles;
[0010] S2. The aqueous dispersion of Fe3O4-polyethylene glycol particles was added to a mixed solution of ethanol, ammonium hydroxide and octadecyltrimethylammonium bromide, and tetraethoxysilane was added dropwise after stirring. After the reaction was completed, the catalyst precursor was collected by magnetic absorption;
[0011] S3. The catalyst precursor obtained in S2 is added to a pure aqueous solution of trisulfomethane, sulfonated under reflux, the product is washed after cooling, and the product is dried in vacuo to obtain a catalyst;
[0012] S4. The catalyst obtained in step S3 and the carboxylic anhydride are mixed and insulated to obtain an insulated reaction liquid, and the tea ketone is added dropwise to the insulated reaction liquid, and reacted to obtain a reaction completed liquid, wherein the molar ratio of the tea ketone to the carboxylic anhydride is 1:(2.4-2.8), and the mass of the catalyst is 0.8-1.1% of the mass of the carboxylic anhydride;
[0013] S5. The reaction solution in step S4 is cooled to allow the product to crystallize, and then the reaction solution is filtered after cooling, and the catalyst is recovered by magnetic absorption to obtain a filtrate of a crude product cake, unreacted raw materials, carboxylic acid and by-products;
[0014] S6. The crude product cake of step S5 is eluted with a saturated carboxylic acid solution of 2,3,5-trimethylhydroquinone diester to obtain a crude product eluted filter cake and an eluent, and the crude product eluted filter cake is washed with water and dried to obtain a product;
[0015] S7. The filtrate of step S5 is mixed with the eluent of step S6, and the carboxylic acid is removed by distillation to obtain a circulating liquid; after discharging 5% of the circulating liquid and adding carboxylic anhydride and the catalyst recovered in step S5, the circulating liquid is returned to step S4.
[0016] Furthermore, the temperature for crystallizing the product in step S5 is -20-25°C, preferably -4-10°C.
[0017] Furthermore, the preparation method of the hydrophilic Fe3O4 particles is to dissolve ferric chloride hexahydrate, trisodium citrate and sodium acetate in ethylene glycol under magnetic stirring, then transfer the obtained solution to an autoclave, heat it at 10MPa-100Mpa, 100-200°C for 5-10 hours, and then cool it to room temperature. The product is washed with deionized water and ethanol for 3 times respectively, and the mass ratio of ferric chloride hexahydrate, trisodium citrate and sodium acetate is (1:3):1:(2-6).
[0018] Furthermore, in step S1, the heating temperature is 45-55° C., the stirring time is 60-80 min, the ammonia solution is added until the pH reaches 7.5, and the stirring is carried out for 1.5-2.5 h after the ammonia solution is added.
[0019] Furthermore, in step S2, the molar ratio of tetraethoxysilane: octadecyltrimethylammonium bromide: ammonium hydroxide: ethanol: water is 1: (0.055-0.065): (1.5-2): (240-260): (180-210), the mass ratio of the Fe3O4-polyethylene glycol particles to tetraethoxysilane is 1: (2.6-2.8), and the reaction time is 7-8h.
[0020] Furthermore, in step S3, the mass ratio of water: trisulfone: catalyst precursor is (20-25): (6-7): 1, the sulfonation time is 1-1.5 hours, the drying temperature is 90-100° C., and the drying time is 3-4 hours.
[0021] Furthermore, in step S4, the insulation temperature is 0-60° C., the insulation time is 0-60 min, the reaction temperature is 30-90° C., and the reaction time is 3-10 h.
[0022] Furthermore, the product obtained after washing and drying in step S6 is recrystallized with an inert solvent such as hydrocarbon or ether to improve the purity of the product, and the washing waste liquid is separated and recovered by distillation.
[0023] Furthermore, in step S7, the circulating liquid reaches saturation due to the accumulation of by-products, so it is necessary to discharge a portion of the circulating liquid to keep the concentration of the by-products within an acceptable range, and to add the acylating agent in time to compensate for its amount in the circulation.
[0024] The beneficial effects of this application are:
[0025] 1. The catalyst system used in the present invention is based on the modification of hydrophilic Fe3O4 particles and the composite with mesoporous silica. Through sulfonation, it has the catalytic effect of rearrangement acylation, which not only avoids the corrosive problem of traditional strong acid catalysts, significantly improves the safety of the production process, but also has a high degree of selectivity and acts as an antioxidant, because it reduces the occurrence of side reactions, thereby improving the yield and purity of the target product. More importantly, the catalyst can be recycled through magnetic recovery, greatly reducing production costs and environmental burdens.
[0026] 2. The present application not only effectively controls the concentration of by-products and prevents them from accumulating to unacceptable levels by continuously using the circulating liquid and adjusting its composition in a timely manner, but also balances the consumption in the circulation system by timely supplementing the acylating agent. In addition, the method does not require real-time separation of the by-products of the reaction. By continuously accumulating and then combining them for recovery, this strategy not only improves the utilization efficiency of resources, but also reduces waste emissions. DETAILED DESCRIPTION
[0027] The technical scheme of the present invention and its effects are further described below by specific examples. The following examples are only used to illustrate the content of the present invention and are not used to limit the protection scope of the present invention. Simple changes made to the present invention by applying the concept of the present invention are all within the scope of the protection claimed by the present invention.
[0028] The equipment used in the preparation method of the present invention can be the well-known equipment in the art. The raw materials used in the present invention are commercially available unless otherwise specified. Example 1
[0029] S1. Ferric chloride hexahydrate, trisodium citrate and sodium acetate were dissolved in ethylene glycol under magnetic stirring, and then the obtained solution was transferred to an autoclave, heated at 100 MPa and 100°C for 5 hours, and then cooled to room temperature. The product was washed 3 times with deionized water and ethanol respectively, and the mass ratio of ferric chloride hexahydrate, trisodium citrate and sodium acetate was 1:1:2; 1.2 g of the prepared hydrophilic Fe3O4 particles were added to 20 mL of pure water, and 10 mL of polyethylene glycol 3000 solution was added thereto under nitrogen atmosphere and vigorous stirring, and the resulting mixture was stirred at 50°C for 60 minutes, and then 28% ammonia water was added under stirring until the pH was 7.5, and the mixture was continued to be stirred at 50°C for 2 hours, and then the precipitate was collected by centrifugation at 6000 rpm for 30 minutes at 25°C, and washed 3 times with pure water to remove unreacted polyethylene glycol.
[0030] S2. 70 mL of the aqueous dispersion of Fe3O4-polyethylene glycol particles obtained in step S1, 0.02 g / mL, was added to a mixed solution of 280 mL of anhydrous ethanol, 5 mL of 28% ammonium hydroxide and 0.42 g of octadecyltrimethylammonium bromide, and stirred at 30°C for 15 minutes. Then, 4.0 mL of tetraethoxysilane was added dropwise, and the reaction was allowed to proceed for 8 hours under stirring. The resulting catalyst precursor was separated and collected with a magnet, and then washed with ethanol 6 times.
[0031] S3. Add 6g of trisulfone and 1g of S2 to obtain the catalyst precursor in 25ml of pure water, carry out sulfonation at reflux temperature for 1h, cool to room temperature, wash the product with pure water 3 times, then wash once with tetrahydrofuran and diethyl ether respectively, and finally dry the product in vacuum at 100°C for 3h to obtain the catalyst.
[0032] S4. 80 g of tea ketone, 115 g of acetic anhydride, 1.2 g of catalyst and 100 g of circulating solution are pumped into the reaction vessel every hour. The circulating solution includes 28% 2,3,5-trimethylhydroquinone diester, 20% 3,5-diacetoxyacetophenone and 45% acetic anhydride, and the temperature of the vessel is controlled at 50-55°C.
[0033] S5. Add the reaction solution into a crystallization device and cool it to 4-10°C while stirring. Filter the obtained suspension every 5 hours and recover the catalyst by magnetic attraction to obtain a crude product filter cake, unreacted raw materials, carboxylic acid and a filtrate of by-products.
[0034] S6. Displace the adhering solution by washing with 120 g of a saturated solution of 2,3,5-trimethylhydroquinone diester in acetic acid.
[0035] S7. The filtrate and the rinse liquid are then added to a distillation apparatus to remove acetic acid by distillation, and then 5% of the filtrate is discharged as the bottom product of the distillation, and the remaining filtrate is re-added to the reaction vessel together with 12.3 g of an acylating agent and the catalyst recovered in S5.
[0036] Finally, the solid was dried under vacuum to obtain 2,3,5-trimethylhydroquinone diester with a purity of 98.40% and a product yield of 99.65%. Example 2
[0037] S1. Ferric chloride hexahydrate, trisodium citrate and sodium acetate were dissolved in ethylene glycol under magnetic stirring, and then the obtained solution was transferred to an autoclave, heated at 10 MPa and 200°C for 10 hours, and then cooled to room temperature. The product was washed 3 times with deionized water and ethanol respectively, and the mass ratio of ferric chloride hexahydrate, trisodium citrate and sodium acetate was 3:1:6; 2 g of the prepared hydrophilic Fe3O4 particles were added to 20 mL of pure water, and 10 mL of polyethylene glycol 3000 solution was added thereto under nitrogen atmosphere and vigorous stirring, and the resulting mixture was stirred at 55°C for 70 minutes, and then 28% ammonia water was added under stirring until the pH was 7.5, and the mixture was continued to be stirred at 55°C for 2 hours, and then the precipitate was collected by centrifugation at 6000 rpm for 30 minutes at 25°C, and washed 3 times with pure water to remove unreacted polyethylene glycol.
[0038] S2. 80 mL of the aqueous dispersion of Fe3O4-polyethylene glycol particles obtained in step S1, 0.02 g / mL, was added to a mixed solution of 280 mL of anhydrous ethanol, 5 mL of 28% ammonium hydroxide and 0.37 g of octadecyltrimethylammonium bromide, and stirred at 30°C for 15 minutes. Then, 5.0 mL of tetraethoxysilane was added dropwise, and the reaction was allowed to proceed for 7 hours under stirring. The resulting catalyst precursor was separated and collected with a magnet, and then washed with ethanol 6 times.
[0039] S3. Add 6g of trisulfone and 1g of S2 to obtain the catalyst precursor in 25ml of pure water, carry out sulfonation at reflux temperature for 1h, cool to room temperature, wash the product with pure water 3 times, then wash once with tetrahydrofuran and diethyl ether respectively, and finally dry the product in vacuum at 100°C for 3h to obtain the catalyst.
[0040] S4. 80 g of tea ketone, 115 g of acetic anhydride, 1.2 g of catalyst and 100 g of circulating solution are pumped into the reaction vessel every hour. The circulating solution includes 28% 2,3,5-trimethylhydroquinone diester, 20% 3,5-diacetoxyacetophenone and 45% acetic anhydride, and the temperature of the vessel is controlled at 50-55°C.
[0041] S5. Add the reaction solution into a crystallization device and cool it to 4-10°C while stirring. Filter the obtained suspension every 5 hours and recover the catalyst by magnetic attraction to obtain a crude product filter cake, unreacted raw materials, carboxylic acid and a filtrate of by-products.
[0042] S6. Displace the adhering solution by washing with 120 g of a saturated solution of 2,3,5-trimethylhydroquinone diester in acetic acid.
[0043] S7. The filtrate and the rinse liquid are then added to a distillation apparatus to remove acetic acid by distillation, and then 5% of the filtrate is discharged as the bottom product of the distillation, and the remaining filtrate is re-added to the reaction vessel together with 12.3 g of an acylating agent and the catalyst recovered in S5.
[0044] Finally, the solid was dried under vacuum to obtain 2,3,5-trimethylhydroquinone diester with a purity of 98.38% and a product yield of 99.68%.
[0045] Example 3-11
[0046] The preparation method and synthesis process used in the example are the same as those in Example 1, and the differences and synthesis effects are shown in Table 1.
[0047] Example Cycle times Product yield Product Purity Purity of by-products 3 2 99.64% 98.32% 0.48% 4 3 99.53% 98.03% 0.64% 5 4 99.35% 97.64% 0.83% 6 5 99.14% 97.32% 0.96% 7 6 99.97% 96.81% 1.27% 8 7 99.27% 96.76% 1.64% 9 8 99.51% 96.54% 1.92% 10 9 99.24% 96.21% 2.71% 11 10 99.05% 95.61% 3.69%
[0048] Comparative Example 1
[0049] 15g of concentrated sulfuric acid and 160g of acetic anhydride were added to a 500mL four-necked flask with nitrogen in turn. After keeping the temperature at 50°C for 30min, 80g of tea ketone was added dropwise. After the addition was completed, the temperature was kept for 7h. After the reaction was completed, the reaction solution was placed at 4-10°C for 12h and then filtered under anhydrous conditions to obtain a crude product and a filtrate. The crude product was recrystallized from 30mL of anhydrous ethanol to obtain 40g of 2,3,5-trimethylhydroquinone diester with a purity of 95.3%. The separation yield was 55% relative to the added tea ketone. After adding water to the filtrate, crystals precipitated again, and the secondary filtration crude product and filtrate were obtained by filtration. The secondary filtration crude product was recrystallized from 30mL of anhydrous ethanol to obtain 25g of 2,3,5-trimethylhydroquinone diester with a purity of 81.3%. The separation yield was 31% relative to the added tea ketone.
[0050] Comparative Example 1 does not add hydrophilic Fe3O4 particles composite silica catalyst, and uses concentrated sulfuric acid as a catalyst. It can be seen that according to the existing process, the purities of the 2,3,5-trimethylhydroquinone diester products obtained by two crystallizations are 95.3% and 81.3%, respectively, and the yields are 55% and 31%, respectively, which are far lower than the technical solutions given in the examples. It can be seen that the technical solution provided by the present application makes the reaction highly selective, improves the yield and purity of the target product, and concentrated sulfuric acid cannot be recovered as a catalyst, while the composite catalyst used in the present application can be recycled and reused, reducing production costs.
Claims
1. A method for preparing 2,3,5-trimethylhydroquinone diester, characterized in that: The following steps are involved: S1. Under magnetic stirring, ferric chloride hexahydrate, trisodium citrate and sodium acetate are dissolved in ethylene glycol, and then the obtained solution is transferred to an autoclave, heated at 10MPa-100Mpa, 100-200°C for 5-10 hours, and then cooled to room temperature. The product is washed 3 times with deionized water and ethanol respectively, and the mass ratio of ferric chloride hexahydrate, trisodium citrate and sodium acetate is (1:3):1:(2-6), and hydrophilic Fe3O4 particles are obtained; polyethylene glycol is added to the aqueous dispersion of hydrophilic Fe3O4 particles under a nitrogen atmosphere, and the mass ratio of the hydrophilic Fe3O4 particles to the polyethylene glycol is 0.1-0.2:
1. After heating and stirring, an ammonia solution is added, and the lower layer of precipitate is collected by centrifugation after continued stirring, and Fe3O4-polyethylene glycol particles are obtained after washing; S2. The aqueous dispersion of Fe3O4-polyethylene glycol particles was added to a mixed solution of ethanol, ammonium hydroxide and octadecyltrimethylammonium bromide, and tetraethoxysilane was added dropwise after stirring. After the reaction was completed, the catalyst precursor was collected by magnetic absorption; S3. The catalyst precursor obtained in S2 is added to a pure aqueous solution of trisulfomethane, sulfonated under reflux, the product is washed after cooling, and the product is dried in vacuo to obtain a catalyst; S4. The catalyst obtained in step S3 and the carboxylic anhydride are mixed and insulated to obtain an insulated reaction liquid, and the tea ketone is added dropwise to the insulated reaction liquid, and reacted to obtain a reaction completed liquid, wherein the molar ratio of the tea ketone to the carboxylic anhydride is 1:(2.4-2.8), and the mass of the catalyst is 0.8-1.1% of the mass of the carboxylic anhydride; S5. The reaction solution in step S4 is cooled to allow the product to crystallize, and then the reaction solution is filtered after cooling, and the catalyst is recovered by magnetic absorption to obtain a filtrate of a crude product cake, unreacted raw materials, carboxylic acid and by-products; S6. The crude product cake of step S5 is eluted with a saturated carboxylic acid solution of 2,3,5-trimethylhydroquinone diester to obtain a crude product eluted filter cake and an eluent, and the crude product eluted filter cake is washed with water and dried to obtain a product; S7. The filtrate of step S5 is mixed with the eluent of step S6, and the carboxylic acid is removed by distillation to obtain a circulating liquid; after discharging 5% of the circulating liquid and adding carboxylic anhydride and the catalyst recovered in step S5, the circulating liquid is returned to step S4.
2. The method for preparing 2,3,5-trimethylhydroquinone diester according to claim 1, characterized in that: The temperature for crystallizing the product in step S5 is -20 to 25°C.
3. The method for preparing 2,3,5-trimethylhydroquinone diester according to claim 1, characterized in that: In step S1, the heating temperature is 45-55° C., the stirring time is 60-80 min, and the ammonia solution is added until the pH reaches 7.
5. After adding the ammonia solution, stirring is performed for 1.5-2.5 h.
4. The method for preparing 2,3,5-trimethylhydroquinone diester according to claim 1, characterized in that: In step S2, the molar ratio of tetraethoxysilane: octadecyltrimethylammonium bromide: ammonium hydroxide: ethanol: water is 1: (0.055-0.065): (1.5-2): (240-260): (180-210), the mass ratio of the Fe3O4-polyethylene glycol particles to tetraethoxysilane is 1: (2.6-2.8), and the reaction time is 7-8h.
5. The method for preparing 2,3,5-trimethylhydroquinone diester according to claim 1, characterized in that: In step S3, the mass ratio of water: trisulfone: catalyst precursor is (20-25): (6-7): 1, the sulfonation time is 1-1.5 hours, the drying temperature is 90-100° C., and the drying time is 3-4 hours.
6. The method for preparing 2,3,5-trimethylhydroquinone diester according to claim 1, characterized in that: In step S4, the molar ratio of tea ketone to carboxylic anhydride is 1:(2.4-2.8), the mass of the catalyst is 0.8-1.1% of the mass of the carboxylic anhydride, the insulation temperature is 0-60°C, the insulation time is 0-60min, the reaction temperature is 30-90°C, and the reaction time is 3-10h.