A kind of high temperature resistant plastic and preparation method thereof
By introducing graphene oxide composite support filler and modified cerium dioxide nanofiller into polyphenylene sulfide, combined with KH570 silane coupling agent and carboxymethyl chitosan, the brittleness and oxidation problems of polyphenylene sulfide materials are solved. , significantly improves its toughness, impact resistance and oxidation resistance, and extends its service life.
Patent Information
- Application Number
- CN202410638884.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-22
- Publication Date
- 2024-12-20
- Estimated Expiration
- 2044-05-22
AI Technical Summary
Polyphenylene sulfide materials have problems such as high brittleness, poor toughness, poor impact resistance, and easy oxidation, resulting in reduced performance and shortened service life.
The dispersion and crosslinking structure of the material are improved by combining graphene oxide composite support filler and modified ceria nanofiller with polyphenylene sulfide through the introduction of KH570 silane coupling agent and carboxymethyl chitosan. Strengthen toughness and heat resistance, and improve oxidation resistance through end carboxylic nitrile rubber.
It significantly improves the toughness, impact resistance and oxidation resistance of polyphenylene sulfide, extends the service life, and maintains excellent heat resistance in high-temperature environments, reducing the occurrence of aging.
Smart Images

Figure CN118620383B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and specifically refers to a high temperature resistant plastic and a preparation method thereof. Background Art
[0002] Compared with traditional materials such as metal and glass, ordinary plastics have the disadvantage of low heat resistance, which often limits their use in high-temperature occasions. Therefore, in order to meet the needs of market development, many high-temperature resistant engineering plastics have emerged; high-temperature resistant engineering plastics themselves have a special structure and can still maintain high mechanical properties under high temperature conditions, such as polyphenylene ether, polyphenylene sulfide, polysulfone and other materials.
[0003] Polyphenylene sulfide is a special plastic with excellent properties. It is known as one of the six major engineering plastics and one of the eight major aerospace materials. Its structure is a repeating structural unit consisting of benzene rings and sulfur atoms alternately connected. The main molecular chain contains sulfur benzene. The rigid structure makes it hard, low in density and has good mechanical properties. The relative density of polyphenylene sulfide is 1.36, and its melting point is 280°C. It appears as white powder or granules, which is hard and brittle, with high crystallinity and strong melt viscosity. Therefore, it can bond well with many metal and non-metal materials, and can also bond with many polymer materials.
[0004] The existing technology currently has the following problems:
[0005] Polyphenylene sulfide has the disadvantages of high brittleness, poor toughness and poor impact resistance, which is not conducive to processing and molding. At the same time, polyphenylene sulfide is easily oxidized, showing aging phenomena such as cracking, resulting in performance degradation and shortened service life. Summary of the invention
[0006] In view of the above situation, in order to overcome the defects of the prior art, the present invention proposes a high temperature resistant plastic, comprising the following components in parts by weight: 20-30 parts of graphene oxide composite carrier filler, 10-20 parts of modified cerium dioxide nanofiller, 70-80 parts of polyphenylene sulfide, 8-10 parts of dibutyl phthalate, and 5-8 parts of polytetrafluoroethylene.
[0007] The graphene oxide composite carrier filler comprises the following components in parts by weight: 30-50 parts of KH570 type silane coupling agent, 3-6 parts of graphene oxide, and 20-30 parts of carboxyl-terminated nitrile rubber.
[0008] The modified cerium dioxide nanofiller comprises the following components in parts by weight: 2-4 parts of carboxymethyl chitosan and 10-20 parts of cerium nitrate hexahydrate.
[0009] The method for preparing the graphene oxide composite carrier filler specifically comprises the following steps:
[0010] (1) 0.3 g of graphene oxide was added to 25 mL of anhydrous ethanol. Graphene oxide has good strength and flexibility due to its honeycomb structure. It can form a composite material with polymer materials to enhance toughness and improve heat resistance. Ultrasonic dispersion was carried out in a water bath for 30-60 min. The suspension was transferred to a three-necked flask, and KH570 silane coupling agent was added. Nitrogen was introduced for protection. The reaction was condensed and refluxed at 100-110 ° C for 10-12 h. KH570 was successfully grafted onto the surface of graphene oxide, effectively reducing the graphene oxide. The self-agglomeration improves the dispersibility of graphene oxide in polyphenylene sulfide materials, has better interface properties, significantly enhances tensile strength, fracture toughness and heat resistance, improves the shortcomings of large brittleness and poor toughness, and the obtained mixed solution is filtered, and then washed 3-5 times with toluene solution, 70-80% ethanol solution by mass fraction, and deionized water in sequence, each time using 50 mL, and the obtained filter cake is freeze-dried at a freeze-drying temperature of -30°C to -50°C and a freeze-drying time of 2-3d to obtain KH570 modified graphene oxide;
[0011] (2) adding the KH570 modified graphene oxide described in step (1) to the carboxyl-terminated nitrile rubber, stirring for 3-5 min using a high-speed homogenizer at 130-160° C., with a stirring speed of 10000-20000 rpm, and then curing at 80-90° C. for 1-2 h and at 100-120° C. for 2-3 h, so that the carboxyl groups in the carboxyl-terminated nitrile rubber react with the epoxy groups in the KH570 modified graphene oxide, and the nitrile copolymer segments are embedded in the cross-linked structure, which plays a toughening role, thereby obtaining a graphene oxide composite carrier filler;
[0012] Preferably, in step (1), the amount of KH570 silane coupling agent added is 1.5-5 g, and the hydrolyzed groups of the KH570 silane coupling agent form an organic adsorption layer on the surface of graphene oxide, further improving the heat resistance;
[0013] Preferably, in step (2), the amount of carboxyl-terminated nitrile rubber added is 1-3 g. Carboxyl-terminated nitrile rubber has good resistance to ultraviolet rays and sunlight exposure, and is not prone to aging reactions such as color change, embrittlement and breakage.
[0014] The preparation method of the modified cerium dioxide nanofiller specifically comprises the following steps:
[0015] Dissolve 1-2g of carboxymethyl chitosan in 60mL of distilled water for standby use, prepare 100mL of cerium nitrate hexahydrate solution with a mass fraction of 5-10%, then add the carboxymethyl chitosan solution to mix, control the temperature at 65-75°C, stir for 5-6h, and synthesize cerium dioxide nanoparticles with carboxymethyl chitosan, which is environmentally friendly and pollution-free. The introduction of carboxymethyl chitosan improves the antioxidant property and has good ultraviolet absorption ability. It can also form a composite system through the hydrogen bonding of the carboxyl group, increase cross-linking, and enhance toughness and heat resistance. After stirring, the reaction product is cooled to room temperature and centrifuged at a centrifugal speed of 8 000-10000rpm, centrifugal time 5-10min, remove the supernatant, wash the obtained precipitate with anhydrous ethanol and distilled water for 2-3 times, dry, the drying temperature is 50-60℃, the drying time is 8-12h, and then calcined, the calcination temperature is 500-600℃, the calcination time is 1-2h. Too low temperature and short time are not conducive to the crystallinity of cerium dioxide particles, resulting in less carboxymethyl chitosan on its surface, while too high temperature and too long time also increase the decomposition of carboxymethyl chitosan, which is not conducive to enhancing the antioxidant properties and the hydrogen bonding effect of the carboxyl group, thereby obtaining a modified cerium dioxide nanofiller.
[0016] The present invention also provides a method for preparing a high temperature resistant plastic, which specifically comprises the following steps:
[0017] S1. Mixing the graphene oxide composite carrier filler and the modified cerium dioxide nanofiller, adding them into an extruder for melt extrusion, granulation, and controlling the melt extrusion temperature at 150-200° C. The graphene oxide composite carrier filler can reduce the agglomeration of nanoparticles of the modified cerium dioxide nanofiller. The modified cerium dioxide nanofiller is a rigid particle that absorbs impact energy through plastic deformation when subjected to external force. The improvement of its dispersibility is conducive to enhancing uniform heat resistance. The two are synergistically conducive to enhancing the heat resistance, toughness and oxidation resistance of the composite, thereby obtaining a composite filler masterbatch;
[0018] S2, polyphenylene sulfide, the composite filler masterbatch described in step S1, dibutyl phthalate, and polytetrafluoroethylene are mixed at a mixing speed of 800-1000rpm and a mixing time of 5-15min, wherein dibutyl phthalate is used as a plasticizer and polytetrafluoroethylene is used as a lubricant to enhance the processing properties of polyphenylene sulfide and the composite filler masterbatch, the mixture is placed in an extruder and extruded to obtain a feed material at an extrusion temperature of 280-320°C, and then the feed material is injection molded in an injection molding machine at an injection molding temperature of 300-320°C, an injection molding pressure of 100-200MPa, and a holding time of 10-80s to obtain a high temperature resistant plastic;
[0019] Preferably, in step S1, during the mixing process, the mixing speed is 1000-2000 rpm, and the mixing time is 10-20 min. The uniform mixing of the components provides a basic condition for the graphene oxide composite carrier to better uniformly load the modified cerium dioxide nanofiller.
[0020] The beneficial effects achieved by the present invention are as follows:
[0021] The invention prepares a high-temperature resistant plastic by adding a graphene oxide composite carrier filler and a modified cerium dioxide nanofiller into a polyphenylene sulfide material. The plastic has excellent heat resistance, and at the same time, the toughness, impact resistance and oxidation resistance are enhanced, so that the plastic is not easy to age, the mechanical properties are effectively improved, and the service life is extended. In the graphene oxide composite carrier filler, the KH570 type silane coupling agent modifies the graphene oxide, so that the uniform dispersion state of the carrier filler is improved, and the plastic has good interface compatibility. The addition of the carboxyl-terminated nitrile rubber embeds the cross-linked structure of the modified graphene oxide. The nitrile copolymer chain segment enhances toughness and strength, improves mechanical properties, and also gives the carrier filler good antioxidant properties, reduces the oxidation caused by ultraviolet rays and light, thereby improving the aging phenomenon of polyphenylene sulfide. At the same time, the good compatibility effect is conducive to further exerting the heat resistance, toughness and impact resistance of the carrier filler; the modified cerium dioxide nanofiller, as a rigid particle, disperses and absorbs external impacts to prevent the expansion of cracks, enhance toughness and strength, and thus improve toughness and impact resistance. Among them, carboxymethyl chitosan is attached to the cerium dioxide nanofiller The surface of the particles improves the antioxidant activity of cerium dioxide, has good ultraviolet absorption ability, effectively inhibits the oxidation process, and also increases biocompatibility and degradability; the carboxymethyl chitosan in the modified cerium dioxide nanofiller forms a composite system with the graphene oxide composite carrier filler through hydrogen bonding, increases its cross-linking degree, enriches the network structure of the graphene oxide composite carrier filler, is beneficial to the compatibility effect with polyphenylene sulfide, and effectively enhances the toughness, impact resistance and other mechanical properties, while the graphene oxide composite carrier filler can load the modified cerium dioxide nanofiller, reducing the modified The agglomeration of cerium dioxide nanofiller increases its dispersion uniformity, which is also conducive to the uniform and stable performance of its heat resistance, and also plays a positive role in improving toughness and impact resistance. The excellent high temperature resistance can also effectively inhibit oxidation caused by high temperature environment and reduce the aging of plastics. The present invention uses graphene oxide composite carrier filler, modified cerium dioxide nanofiller, polyphenylene sulfide, dibutyl phthalate and polytetrafluoroethylene to make a high temperature resistant plastic, which enhances heat resistance, improves toughness and impact resistance, and also has antioxidant properties, effectively reduces the occurrence of aging and prolongs service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a scanning electron microscope image of the graphene oxide composite carrier filler prepared in Example 1 of the present invention;
[0023] Figure 2 This is a scanning electron microscope image of the modified cerium dioxide nanofiller prepared in Example 1 of the present invention;
[0024] Figure 3 The heat deformation temperature results of Examples 1-4 and Comparative Examples 1-3 of the present invention are shown in FIG.
[0025] Figure 4 The mechanical properties of Examples 1-4 and Comparative Examples 1-3 of the present invention are shown in FIG.
[0026] Figure 5 It is a graph showing the anti-aging results of Examples 1-4 of the present invention and Comparative Examples 1-3. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0028] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0029] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0030] The sources of the reagents used in the examples are as follows:
[0031] Graphene oxide CASNo:7782-42-5, brand Aladdin, product number G139803;
[0032] KH570 silane coupling agent brand Qufu Chenguang, item number KH570;
[0033] Carboxyl-terminated nitrile rubber brand Fusion, item number FZ-0141374-100g;
[0034] Toluene CAS No: 108-88-3, brand Innochem, product number 105076-A500ML;
[0035] Carboxymethyl chitosan CAS No: 83512-85-0, brand Apinno, product number GC86327;
[0036] Cerium nitrate hexahydrate CAS No: 10294-41-4, brand Innochem, product number A22708;
[0037] Polyphenylene sulfide CAS No: 25212-74-2, brand Sigma-aldrich, product number 182354-100G;
[0038] Dibutyl phthalate CAS No: 84-74-2, brand Innochem, product number A84622;
[0039] Polytetrafluoroethylene CAS No: 9002-84-0, brand Acros, item number 178931000;
[0040] Anhydrous ethanol CAS No: 64-17-5, brand Innochem, product number G00004.
[0041] Example 1
[0042] This embodiment proposes a high temperature resistant plastic, comprising the following components in parts by weight: 30 parts of graphene oxide composite carrier filler, 20 parts of modified cerium dioxide nanofiller, 80 parts of polyphenylene sulfide, 10 parts of dibutyl phthalate, and 8 parts of polytetrafluoroethylene.
[0043] The graphene oxide composite carrier filler comprises the following components in parts by weight: 50 parts of KH570 type silane coupling agent, 3 parts of graphene oxide, and 30 parts of carboxyl-terminated nitrile rubber.
[0044] The modified cerium dioxide nanofiller comprises the following components in parts by weight: 4 parts of carboxymethyl chitosan and 20 parts of cerium nitrate hexahydrate.
[0045] The preparation method of the graphene oxide composite carrier filler specifically comprises the following steps:
[0046] (1) 0.3 g of graphene oxide was added to 25 mL of anhydrous ethanol. Graphene oxide has good strength and flexibility due to its honeycomb structure. It can form a composite material with polymer materials to enhance toughness and improve heat resistance. Ultrasonic dispersion was carried out in a water bath for 60 min. The suspension was transferred to a three-necked flask, and KH570 silane coupling agent was added. Nitrogen was introduced for protection. The reaction was condensed and refluxed at 110 ° C for 12 h. The amount of KH570 silane coupling agent added was 5 g. The hydrolyzed groups of KH570 silane coupling agent formed an organic adsorption layer on the surface of graphene oxide, which further improved the heat resistance. Thermal properties, KH570 was successfully grafted onto the surface of graphene oxide, effectively reducing the self-agglomeration of graphene oxide, improving the dispersibility of graphene oxide in polyphenylene sulfide materials, having better interface properties, significantly enhancing tensile strength, fracture toughness and heat resistance, and improving the shortcomings of large brittleness and poor toughness. The obtained mixed solution was filtered, and then washed 5 times with toluene solution, 80% ethanol solution by mass, and deionized water in turn, each time with 50 mL, and the obtained filter cake was freeze-dried at a freeze-drying temperature of -50 ° C and a freeze-drying time of 3 days to obtain KH570 modified graphene oxide;
[0047] (2) Adding the KH570 modified graphene oxide described in step (1) to the carboxyl-terminated nitrile rubber, the amount of the carboxyl-terminated nitrile rubber added is 3 g. The carboxyl-terminated nitrile rubber has good resistance to ultraviolet rays and sunlight exposure, and is not prone to aging reactions such as color change, embrittlement and fracture. Stirring the graphene oxide with a high-speed homogenizer at 160° C. for 5 min at a stirring speed of 20,000 rpm, and then curing the graphene oxide with a carboxyl group in the carboxyl-terminated nitrile rubber and an epoxy group in the KH570 modified graphene oxide, embedding the nitrile copolymer chain segment in the cross-linked structure, thereby achieving a toughening effect, thereby obtaining a graphene oxide composite carrier filler.
[0048] The preparation method of the modified cerium dioxide nanofiller specifically comprises the following steps:
[0049] Dissolve 2g of carboxymethyl chitosan in 60mL of distilled water for standby use, prepare 100mL of cerium nitrate hexahydrate solution with a mass fraction of 10%, then add the carboxymethyl chitosan solution to mix, control the temperature at 75°C, stir for 6h, and synthesize cerium dioxide nanoparticles with carboxymethyl chitosan, which is environmentally friendly and pollution-free. The introduction of carboxymethyl chitosan improves the antioxidant property and has good ultraviolet absorption ability. It can also form a composite system through the hydrogen bonding of the carboxyl group, increase cross-linking, and enhance toughness and heat resistance. After the stirring is completed, the reaction product is cooled to room temperature and centrifuged. The centrifugal speed is 10000rpm, the centrifugal time is 10min, the supernatant is removed, and the obtained precipitate is washed 3 times with anhydrous ethanol and distilled water respectively, dried at 60℃ for 12h, and then calcined at 600℃ for 2h. Too low temperature and short time are not conducive to the crystallinity of cerium dioxide particles, resulting in less carboxymethyl chitosan on its surface, while too high temperature and too long time also increase the decomposition of carboxymethyl chitosan, which is not conducive to enhancing the antioxidant properties and the hydrogen bonding effect of the carboxyl group, thereby obtaining a modified cerium dioxide nanofiller.
[0050] This embodiment provides a method for preparing a high temperature resistant plastic, which specifically includes the following steps:
[0051] S1. Mixing graphene oxide composite carrier filler and modified cerium dioxide nanofiller. During the mixing process, the mixing speed is 2000rpm and the mixing time is 20min. The uniform mixing of the components provides a basic condition for the graphene oxide composite carrier to better uniformly load the modified cerium dioxide nanofiller. Adding the graphene oxide composite carrier filler to the extruder for melt extrusion and granulation, the melt extrusion temperature is controlled at 200°C. The graphene oxide composite carrier filler can reduce the agglomeration of nanoparticles of the modified cerium dioxide nanofiller. The modified cerium dioxide nanofiller is a rigid particle. When subjected to external force, it absorbs impact energy through plastic deformation. The improvement of its dispersibility is conducive to enhancing uniform heat resistance. The synergy of the two is conducive to enhancing the heat resistance, toughness and oxidation resistance of the composite, and obtaining a composite filler masterbatch;
[0052] S2. Mix polyphenylene sulfide, the composite filler masterbatch described in step S1, dibutyl phthalate, and polytetrafluoroethylene at a mixing speed of 1000 rpm and a mixing time of 15 min. Dibutyl phthalate is used as a plasticizer and polytetrafluoroethylene is used as a lubricant to enhance the processing properties of polyphenylene sulfide and the composite filler masterbatch. The mixture is extruded in an extruder to obtain a feed material at an extrusion temperature of 320° C. The feed material is then injection molded in an injection molding machine at an injection molding temperature of 320° C., an injection molding pressure of 200 MPa, and a holding time of 80 s to obtain a high temperature resistant plastic.
[0053] In this example, the prepared graphene oxide composite carrier filler and modified cerium dioxide nanofiller were subjected to scanning electron microscopy to observe their microscopic morphology. Figure 1 This is a SEM image of the graphene oxide composite carrier filler prepared in Example 1 magnified 400 times. Figure 2 This is a SEM image of the modified cerium dioxide nanofiller prepared in Example 1 magnified 1000 times, as shown in FIG. Figure 1 The graphene oxide composite carrier filler prepared in this embodiment presents a cross-linked toughening structure, such as Figure 2 The modified cerium dioxide nanofiller prepared in this embodiment is a nanoparticle with a rough surface.
[0054] Example 2
[0055] This embodiment proposes a high temperature resistant plastic, comprising the following components in parts by weight: 20 parts of graphene oxide composite carrier filler, 10 parts of modified cerium dioxide nanofiller, 70 parts of polyphenylene sulfide, 8 parts of dibutyl phthalate, and 5 parts of polytetrafluoroethylene.
[0056] The graphene oxide composite carrier filler comprises the following components in parts by weight: 30 parts of KH570 type silane coupling agent, 6 parts of graphene oxide, and 20 parts of carboxyl-terminated nitrile rubber.
[0057] The modified cerium dioxide nanofiller comprises the following components in parts by weight: 2 parts of carboxymethyl chitosan and 10 parts of cerium nitrate hexahydrate.
[0058] The preparation method of the graphene oxide composite carrier filler specifically comprises the following steps:
[0059] (1) 0.3 g of graphene oxide was added to 25 mL of anhydrous ethanol. Graphene oxide has good strength and flexibility due to its honeycomb structure. It can form a composite material with polymer materials to enhance toughness and improve heat resistance. Ultrasonic dispersion was carried out in a water bath for 30 min. The suspension was transferred to a three-necked flask, and KH570 silane coupling agent was added. Nitrogen was introduced for protection. The reaction was condensed and refluxed at 100 ° C for 10 h. The amount of KH570 silane coupling agent added was 1.5 g. The hydrolyzed groups of KH570 silane coupling agent formed an organic adsorption layer on the surface of graphene oxide, which further improved the Heat resistance, KH570 was successfully grafted onto the surface of graphene oxide, effectively reducing the self-agglomeration of graphene oxide, improving the dispersibility of graphene oxide in polyphenylene sulfide materials, having better interface properties, significantly enhancing tensile strength, fracture toughness and heat resistance, and improving the shortcomings of large brittleness and poor toughness. The obtained mixed solution was filtered, and then rinsed 3 times with toluene solution, 70% ethanol solution by mass, and deionized water in sequence, each time with an amount of 50 mL, and the obtained filter cake was freeze-dried at a freeze-drying temperature of -30 ° C and a freeze-drying time of 2 days to obtain KH570 modified graphene oxide;
[0060] (2) Adding the KH570 modified graphene oxide described in step (1) to the carboxyl-terminated nitrile rubber, the amount of the carboxyl-terminated nitrile rubber added is 1 g. The carboxyl-terminated nitrile rubber has good resistance to ultraviolet rays and sunlight exposure, and is not prone to aging reactions such as color change, embrittlement and fracture. Stirring for 3 minutes at 130° C. using a high-speed homogenizer at a stirring speed of 10,000 rpm, and then curing at 80° C. for 1 hour and at 100° C. for 2 hours, the carboxyl groups in the carboxyl-terminated nitrile rubber react with the epoxy groups in the KH570 modified graphene oxide, and the nitrile copolymer segments are embedded in the cross-linked structure, which plays a toughening role, thereby obtaining a graphene oxide composite carrier filler.
[0061] The preparation method of the modified cerium dioxide nanofiller specifically comprises the following steps:
[0062] 1g of carboxymethyl chitosan was dissolved in 60mL of distilled water for standby use, and then 100mL of cerium nitrate hexahydrate solution with a mass fraction of 5% was prepared, and then the carboxymethyl chitosan solution was added for mixing, the temperature was controlled at 65°C, and stirred for 5h. The cerium dioxide nanoparticles were synthesized with carboxymethyl chitosan, which was environmentally friendly and pollution-free. The introduction of carboxymethyl chitosan improved the antioxidant property and had good ultraviolet absorption ability. It could also form a composite system through the hydrogen bonding of the carboxyl group, increase the crosslinking property, and enhance the toughness and heat resistance. After the stirring was completed, the reaction product was cooled to room temperature and centrifuged. , centrifugal speed 8000rpm, centrifugal time 5min, remove the supernatant, wash the precipitate twice with anhydrous ethanol and distilled water respectively, dry, drying temperature 50℃, drying time 8h, and then calcination, calcination temperature 500℃, calcination time 1h. Too low temperature and short time are not conducive to the crystallinity of cerium dioxide particles, resulting in less carboxymethyl chitosan on its surface, while too high temperature and too long time also increase the decomposition of carboxymethyl chitosan, which is not conducive to enhancing the antioxidant properties and the hydrogen bonding effect of the carboxyl group, and obtain modified cerium dioxide nanofiller.
[0063] This embodiment provides a method for preparing a high temperature resistant plastic, which specifically includes the following steps:
[0064] S1. Mixing graphene oxide composite carrier filler and modified cerium dioxide nanofiller. During the mixing process, the mixing speed is 1000 rpm and the mixing time is 10 min. The uniform mixing of the components provides a basic condition for the graphene oxide composite carrier to better uniformly load the modified cerium dioxide nanofiller. Adding the graphene oxide composite carrier filler to the extruder for melt extrusion and granulation, the melt extrusion temperature is controlled at 150°C. The graphene oxide composite carrier filler can reduce the agglomeration of nanoparticles of the modified cerium dioxide nanofiller. The modified cerium dioxide nanofiller is a rigid particle. When subjected to external force, it absorbs impact energy through plastic deformation. The improvement of its dispersibility is conducive to enhancing uniform heat resistance. The synergy of the two is conducive to enhancing the heat resistance, toughness and oxidation resistance of the composite, and obtaining a composite filler masterbatch;
[0065] S2. Mix polyphenylene sulfide, the composite filler masterbatch described in step S1, dibutyl phthalate, and polytetrafluoroethylene at a mixing speed of 800 rpm and a mixing time of 5 min. Dibutyl phthalate is used as a plasticizer and polytetrafluoroethylene is used as a lubricant to enhance the processing properties of polyphenylene sulfide and the composite filler masterbatch. The mixture is extruded in an extruder to obtain a feed material at an extrusion temperature of 280° C. The feed material is then injection molded in an injection molding machine at an injection molding temperature of 300° C., an injection molding pressure of 100 MPa, and a holding time of 10 s to obtain a high temperature resistant plastic.
[0066] Example 3
[0067] This embodiment proposes a high temperature resistant plastic, comprising the following components in parts by weight: 25 parts of graphene oxide composite carrier filler, 18 parts of modified cerium dioxide nanofiller, 75 parts of polyphenylene sulfide, 9 parts of dibutyl phthalate, and 6.5 parts of polytetrafluoroethylene.
[0068] The graphene oxide composite carrier filler comprises the following components in parts by weight: 40 parts of KH570 silane coupling agent, 4.5 parts of graphene oxide, and 25 parts of carboxyl-terminated nitrile rubber.
[0069] The modified cerium dioxide nanofiller comprises the following components in parts by weight: 3 parts of carboxymethyl chitosan and 15 parts of cerium nitrate hexahydrate.
[0070] The preparation method of the graphene oxide composite carrier filler specifically comprises the following steps:
[0071] (1) 0.3 g of graphene oxide was added to 25 mL of anhydrous ethanol. Graphene oxide has good strength and flexibility due to its honeycomb structure. It can form a composite material with polymer materials to enhance toughness and improve heat resistance. Ultrasonic dispersion was carried out in a water bath for 45 min. The suspension was transferred to a three-necked flask, and KH570 silane coupling agent was added. Nitrogen was introduced for protection. The reaction was condensed and refluxed at 105 °C for 11 h. The amount of KH570 silane coupling agent added was 2.7 g. The hydrolyzed groups of KH570 silane coupling agent formed an organic adsorption layer on the surface of graphene oxide, which further improved the heat resistance. Thermal properties, KH570 was successfully grafted onto the surface of graphene oxide, effectively reducing the self-agglomeration of graphene oxide, improving the dispersibility of graphene oxide in polyphenylene sulfide materials, having better interface properties, significantly enhancing tensile strength, fracture toughness and heat resistance, and improving the shortcomings of large brittleness and poor toughness. The obtained mixed solution was filtered, and then washed 4 times with toluene solution, 75% ethanol solution by mass, and deionized water in sequence, each time with an amount of 50 mL, and the obtained filter cake was freeze-dried at a freeze-drying temperature of -40 ° C and a freeze-drying time of 2.5 days to obtain KH570 modified graphene oxide;
[0072] (2) Adding the KH570 modified graphene oxide described in step (1) to the carboxyl-terminated nitrile rubber, the amount of the carboxyl-terminated nitrile rubber added is 1.7 g. The carboxyl-terminated nitrile rubber has good resistance to ultraviolet rays and sunlight exposure, and is not prone to aging reactions such as color change, embrittlement and fracture. The mixture is stirred at 145° C. for 4 min using a high-speed homogenizer at a stirring speed of 15,000 rpm, and then cured at 85° C. for 1.5 h and at 110° C. for 2.5 h. The carboxyl groups in the carboxyl-terminated nitrile rubber react with the epoxy groups in the KH570 modified graphene oxide, and the nitrile copolymer segments are embedded in the cross-linked structure, which plays a toughening role, thereby obtaining a graphene oxide composite carrier filler.
[0073] The preparation method of the modified cerium dioxide nanofiller specifically comprises the following steps:
[0074] 1.5 g of carboxymethyl chitosan was dissolved in 60 mL of distilled water for standby use, and then 100 mL of cerium nitrate hexahydrate solution with a mass fraction of 7.5% was prepared, and then the carboxymethyl chitosan solution was added for mixing, the temperature was controlled at 70 ° C, and stirred for 5.5 h. The cerium dioxide nanoparticles were synthesized with carboxymethyl chitosan, which is environmentally friendly and pollution-free. The introduction of carboxymethyl chitosan improves the antioxidant property and has good ultraviolet absorption ability. It can also form a composite system through the hydrogen bonding of the carboxyl group, increase the cross-linking property, and enhance the toughness and heat resistance. After the stirring is completed, the reaction product is cooled to room temperature and separated. The centrifugal speed was 9000rpm and the centrifugal time was 7.5min. The supernatant was removed and the precipitate was washed twice with anhydrous ethanol and distilled water respectively, dried at 55℃ and 10h, and then calcined at 550℃ and 1.5h. Too low temperature and short time were not conducive to the crystallinity of cerium dioxide particles, resulting in less carboxymethyl chitosan on its surface, while too high temperature and too long time also increased the decomposition of carboxymethyl chitosan, which was not conducive to enhancing the antioxidant properties and the hydrogen bonding effect of the carboxyl group, thereby obtaining a modified cerium dioxide nanofiller.
[0075] This embodiment provides a method for preparing a high temperature resistant plastic, which specifically includes the following steps:
[0076] S1. Mixing graphene oxide composite carrier filler and modified cerium dioxide nanofiller. During the mixing process, the mixing speed is 1500rpm and the mixing time is 15min. The uniform mixing of the components provides a basic condition for the graphene oxide composite carrier to better uniformly load the modified cerium dioxide nanofiller. Adding the graphene oxide composite carrier filler to the extruder for melt extrusion and granulation, the melt extrusion temperature is controlled at 175°C. The graphene oxide composite carrier filler can reduce the agglomeration of nanoparticles of the modified cerium dioxide nanofiller. The modified cerium dioxide nanofiller is a rigid particle. When subjected to external force, it absorbs impact energy through plastic deformation. The improvement of its dispersibility is conducive to enhancing uniform heat resistance. The synergy of the two is conducive to enhancing the heat resistance, toughness and oxidation resistance of the composite, and obtaining a composite filler masterbatch;
[0077] S2. Mix polyphenylene sulfide, the composite filler masterbatch described in step S1, dibutyl phthalate, and polytetrafluoroethylene at a mixing speed of 900 rpm and a mixing time of 10 min. Dibutyl phthalate is used as a plasticizer and polytetrafluoroethylene is used as a lubricant to enhance the processing properties of polyphenylene sulfide and the composite filler masterbatch. The mixture is extruded in an extruder to obtain a feed material at an extrusion temperature of 300° C. The feed material is then injection molded in an injection molding machine at an injection molding temperature of 310° C., an injection molding pressure of 150 MPa, and a holding time of 45 s to obtain a high temperature resistant plastic.
[0078] Example 4
[0079] This embodiment proposes a high temperature resistant plastic, comprising the following components in parts by weight: 20 parts of graphene oxide composite carrier filler, 20 parts of modified cerium dioxide nanofiller, 80 parts of polyphenylene sulfide, 10 parts of dibutyl phthalate, and 8 parts of polytetrafluoroethylene.
[0080] The graphene oxide composite carrier filler comprises the following components in parts by weight: 50 parts of KH570 type silane coupling agent, 3 parts of graphene oxide, and 30 parts of carboxyl-terminated nitrile rubber.
[0081] The modified cerium dioxide nanofiller comprises the following components in parts by weight: 4 parts of carboxymethyl chitosan and 20 parts of cerium nitrate hexahydrate.
[0082] The preparation method of the graphene oxide composite carrier filler specifically comprises the following steps:
[0083] (1) 0.3 g of graphene oxide was added to 25 mL of anhydrous ethanol. Graphene oxide has good strength and flexibility due to its honeycomb structure. It can form a composite material with polymer materials to enhance toughness and improve heat resistance. Ultrasonic dispersion was carried out in a water bath for 30 min. The suspension was transferred to a three-necked flask, and KH570 silane coupling agent was added. Nitrogen was introduced for protection. The reaction was condensed and refluxed at 110 ° C for 10 h. The amount of KH570 silane coupling agent added was 5 g. The hydrolyzed groups of KH570 silane coupling agent formed an organic adsorption layer on the surface of graphene oxide, which further improved the heat resistance. Thermal properties, KH570 was successfully grafted onto the surface of graphene oxide, effectively reducing the self-agglomeration of graphene oxide, improving the dispersibility of graphene oxide in polyphenylene sulfide materials, having better interface properties, significantly enhancing tensile strength, fracture toughness and heat resistance, and improving the shortcomings of large brittleness and poor toughness. The obtained mixed solution was filtered, and then washed 5 times with toluene solution, 80% ethanol solution by mass, and deionized water in sequence, each time with an amount of 50 mL, and the obtained filter cake was freeze-dried at a freeze-drying temperature of -50 ° C and a freeze-drying time of 2 days to obtain KH570 modified graphene oxide;
[0084] (2) Adding the KH570 modified graphene oxide described in step (1) to the carboxyl-terminated nitrile rubber, the amount of the carboxyl-terminated nitrile rubber added is 3 g. The carboxyl-terminated nitrile rubber has good resistance to ultraviolet rays and sunlight exposure, and is not prone to aging reactions such as color change, embrittlement and fracture. Stirring the graphene oxide with a high-speed homogenizer at 160° C. for 3 min at a stirring speed of 20,000 rpm, and then curing at 90° C. for 1 h and at 120° C. for 2 h. The carboxyl groups in the carboxyl-terminated nitrile rubber react with the epoxy groups in the KH570 modified graphene oxide, and the nitrile copolymer segments are embedded in the cross-linked structure, which plays a toughening role, thereby obtaining a graphene oxide composite carrier filler.
[0085] The preparation method of the modified cerium dioxide nanofiller specifically comprises the following steps:
[0086] 2g of carboxymethyl chitosan was dissolved in 60mL of distilled water for standby use, and then 100mL of cerium nitrate hexahydrate solution with a mass fraction of 10% was prepared, and then the carboxymethyl chitosan solution was added for mixing, the temperature was controlled at 75°C, and stirred for 5h. The cerium dioxide nanoparticles were synthesized with carboxymethyl chitosan, which was environmentally friendly and pollution-free. The introduction of carboxymethyl chitosan improved the antioxidant property and had good ultraviolet absorption ability. It could also form a composite system through the hydrogen bonding of the carboxyl group, increase the crosslinking property, and enhance the toughness and heat resistance. After the stirring was completed, the reaction product was cooled to room temperature and centrifuged. , centrifugal speed 10000rpm, centrifugal time 5min, remove the supernatant, wash the precipitate with anhydrous ethanol and distilled water for 3 times, dry, drying temperature 60℃, drying time 8h, and then calcination, calcination temperature 600℃, calcination time 1h. Too low temperature and short time are not conducive to the crystallinity of cerium dioxide particles, resulting in less carboxymethyl chitosan on its surface, while too high temperature and too long time also increase the decomposition of carboxymethyl chitosan, which is not conducive to enhancing the antioxidant properties and the hydrogen bonding effect of the carboxyl group, and obtain modified cerium dioxide nanofiller.
[0087] This embodiment provides a method for preparing a high temperature resistant plastic, which specifically includes the following steps:
[0088] S1. Mixing graphene oxide composite carrier filler and modified cerium dioxide nanofiller. During the mixing process, the mixing speed is 2000rpm and the mixing time is 10min. The uniform mixing of the components provides a basic condition for the graphene oxide composite carrier to better uniformly load the modified cerium dioxide nanofiller. Adding the graphene oxide composite carrier filler to the extruder for melt extrusion and granulation, the melt extrusion temperature is controlled at 200°C. The graphene oxide composite carrier filler can reduce the agglomeration of nanoparticles of the modified cerium dioxide nanofiller. The modified cerium dioxide nanofiller is a rigid particle. When subjected to external force, it absorbs impact energy through plastic deformation. The improvement of its dispersibility is conducive to enhancing uniform heat resistance. The synergy of the two is conducive to enhancing the heat resistance, toughness and oxidation resistance of the composite, and a composite filler masterbatch is obtained;
[0089] S2. Mix polyphenylene sulfide, the composite filler masterbatch described in step S1, dibutyl phthalate, and polytetrafluoroethylene at a mixing speed of 1000 rpm and a mixing time of 5 min. Dibutyl phthalate is used as a plasticizer and polytetrafluoroethylene is used as a lubricant to enhance the processing properties of polyphenylene sulfide and the composite filler masterbatch. The mixture is extruded in an extruder to obtain a feed material at an extrusion temperature of 320° C. The feed material is then injection molded in an injection molding machine at an injection molding temperature of 320° C., an injection molding pressure of 200 MPa, and a holding time of 10 s to obtain a high temperature resistant plastic.
[0090] Comparative Example 1
[0091] This comparative example provides a high temperature resistant plastic, which differs from Example 1 in that the high temperature resistant plastic does not contain graphene oxide composite carrier filler; the preparation method of modified cerium dioxide nanofiller is the same as that of Example 1; the preparation method of the high temperature resistant plastic is the same as that of Example 1.
[0092] Comparative Example 2
[0093] This comparative example provides a high temperature resistant plastic, which differs from Example 1 in that the high temperature resistant plastic does not contain modified cerium dioxide nanofiller; the preparation method of the graphene oxide composite carrier filler is the same as that of Example 1; and the preparation method of the high temperature resistant plastic is the same as that of Example 1.
[0094] Comparative Example 3
[0095] This comparative example provides a high temperature resistant plastic, which is different from Example 1 in that the high temperature resistant plastic does not contain graphene oxide composite carrier filler and modified cerium dioxide nanofiller; and the preparation method of the high temperature resistant plastic does not include step S1.
[0096] Experimental Example 1
[0097] Heat resistance test
[0098] Test sample: high temperature resistant plastics prepared in Examples 1-4 and Comparative Examples 1-3.
[0099] Test method: The test sample was subjected to a heat resistance test according to ASTM D-648 standard. During the test, the load was controlled to be 1.82 MPa and the span was 100 mm.
[0100] Figure 3 It is a graph of the heat deformation temperature results of Examples 1-4 and Comparative Examples 1-3; as shown in the figure, the heat deformation temperature of Examples 1-4 is 308-335°C, indicating good heat resistance; the heat deformation temperature of Comparative Examples 1-3 is 215-288°C, indicating poor heat resistance; the high-temperature resistant plastic of Comparative Example 1 does not contain graphene oxide composite carrier filler, cannot reduce the agglomeration of modified cerium dioxide nanofiller, is not conducive to the uniform and stable performance of heat resistance, resulting in poor heat resistance; the high-temperature resistant plastic of Comparative Example 2 does not contain modified cerium dioxide nanofiller, and only contains graphene oxide composite carrier filler as a heat-resistant effective substance, resulting in poor heat resistance; the high-temperature resistant plastic of Comparative Example 3 does not contain graphene oxide composite carrier filler and modified cerium dioxide nanofiller, and the two fillers cannot synergistically exert heat resistance, resulting in poor heat resistance.
[0101] Experimental Example 2
[0102] Mechanical properties test
[0103] Test sample: high temperature resistant plastics prepared in Examples 1-4 and Comparative Examples 1-3.
[0104] Test method: The test sample is injected into a standard specimen prepared by an injection molding machine. During the preparation of the standard specimen by the injection molding machine, the temperature of the first section is 280°C, the temperature of the second section is 310°C, the temperature of the third section is 305°C, and the temperature of the head is 295°C. The mechanical properties are tested, wherein the tensile properties are tested in accordance with the standard GB / T1040-1992, and the impact strength is tested in accordance with the provisions of the standard GB / T1843-1996 to measure the cantilever beam notched impact strength.
[0105] Figure 4 The mechanical properties of Examples 1-4 and Comparative Examples 1-3 are shown in the figure. As shown in the figure, the tensile strength and impact strength of Examples 1-4 are 95.6-100.8MPa and 20.1-22.9KJ / m 2 , indicating strong toughness and impact resistance, excellent mechanical properties; the tensile strength and impact strength of comparative examples 1-3 are 76.2-88.4MPa and 11.3-17.5KJ / m 2 , indicating that the toughness and impact resistance are weak, and the mechanical properties are general; the high-temperature resistant plastic of Comparative Example 1 does not contain graphene oxide composite carrier filler, and only contains modified cerium dioxide nanofiller to play a role, resulting in weak toughness and impact resistance, and general mechanical properties; the high-temperature resistant plastic of Comparative Example 2 does not contain modified cerium dioxide nanofiller, and cannot enrich the network structure of the graphene oxide composite carrier filler through hydrogen bonding, which is not conducive to the compatibility effect with polyphenylene sulfide, and cannot effectively enhance the mechanical properties such as toughness and impact resistance, resulting in weak toughness and impact resistance, and general mechanical properties; the high-temperature resistant plastic of Comparative Example 3 does not contain graphene oxide composite carrier filler and modified cerium dioxide nanofiller, that is, it does not contain rigid particles and does not contain synergistic carriers, and the two cannot synergistically play a toughening and strengthening role, resulting in weak toughness and impact resistance, and general mechanical properties.
[0106] Experimental Example 3
[0107] Aging test
[0108] Test sample: high temperature resistant plastics prepared in Examples 1-4 and Comparative Examples 1-3.
[0109] Test method: The test sample is injected into a standard sample bar by an injection molding machine. During the injection molding process, the temperature of the first section is 280°C, the temperature of the second section is 310°C, the temperature of the third section is 305°C, and the temperature of the head is 295°C. The standard sample bar is then placed in an MTSGB-25 UV aging box and UV-aged for 200 hours. After the test, the mechanical properties are tested. The tensile properties are tested according to the standard GB / T1040-1992, and the impact strength is measured according to the standard GB / T1843-1996. Then, the data in Experimental Example 2 are used as the performance parameters before aging. The mechanical property degradation rate is calculated by the following formula. The greater the mechanical property degradation rate, the worse the aging resistance:
[0110] Tensile strength decrease rate (%) = (tensile strength before aging - tensile strength after aging) / tensile strength before aging × 100%
[0111] Impact strength reduction rate (%) = (impact strength before aging - impact strength after aging) / impact strength before aging × 100%
[0112] Figure 5 The aging resistance results of Examples 1-4 and Comparative Examples 1-3 are shown in the figure; as shown in the figure, the tensile strength decrease rate and impact strength decrease rate of Examples 1-4 are 2.5-4.6% and 3.6-5.7%, respectively, indicating that the aging resistance is good; the tensile strength decrease rate and impact strength decrease rate of Comparative Examples 1-3 are 7.8-16.9% and 10.3-21.8%, respectively, indicating that the aging resistance is poor; the high temperature resistant plastic of Comparative Example 1 does not contain graphene oxide composite carrier filler, does not have the antioxidant properties of terminal carboxyl nitrile rubber, and cannot reduce the agglomeration of modified cerium dioxide nanofiller, limiting The anti-aging effect of the modified cerium dioxide nanofiller results in poor aging resistance; the high-temperature resistant plastic of Comparative Example 2 does not contain modified cerium dioxide nanofiller, does not have ultraviolet absorption ability, and cannot inhibit the aging phenomenon caused by the oxidation process, resulting in poor aging resistance; the high-temperature resistant plastic of Comparative Example 3 does not contain graphene oxide composite carrier filler and modified cerium dioxide nanofiller, that is, it does not contain antioxidant active substances, cannot reduce the oxidation caused by ultraviolet rays and light, and cannot improve heat resistance to reduce oxidation caused by high temperature environment, which is not conducive to inhibiting the aging process, resulting in poor aging resistance.
[0113] The above experimental results show that the heat resistance, mechanical properties and aging resistance of Examples 1-4 of the present invention are significantly better than those of Comparative Examples 1-3. Among them, Example 1 using a graphene oxide composite carrier filler and a modified cerium dioxide nanofiller has better heat resistance, stronger mechanical properties and better aging resistance. The graphene oxide composite carrier filler has good interface compatibility. The addition of terminal carboxyl nitrile rubber enhances toughness and strength, improves mechanical properties, and also gives the carrier filler good antioxidant properties, reduces the oxidation caused by ultraviolet rays and light, thereby improving the aging phenomenon of polyphenylene sulfide; the modified cerium dioxide nanofiller, as a rigid particle, prevents the expansion of cracks by dispersing and absorbing external impacts, enhances toughness and strength, and thereby improves toughness and impact resistance. Carboxymethyl chitosan improves the antioxidant activity of cerium dioxide, has good ultraviolet absorption ability, and effectively inhibits the oxidation process.
[0114] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.
[0115] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A high temperature resistant plastic, characterized in that: The high temperature resistant plastic comprises the following components in parts by weight: 20-30 parts of graphene oxide composite carrier filler, 10-20 parts of modified cerium dioxide nanofiller, 70-80 parts of polyphenylene sulfide, 8-10 parts of dibutyl phthalate, and 5-8 parts of polytetrafluoroethylene; the graphene oxide composite carrier filler comprises the following components in parts by weight: 30-50 parts of KH570 type silane coupling agent, 3-6 parts of graphene oxide, and 20-30 parts of carboxyl-terminated nitrile rubber; the modified cerium dioxide nanofiller comprises the following components in parts by weight: 2-4 parts of carboxymethyl chitosan and 10-20 parts of cerium nitrate hexahydrate.
2. A method for preparing a high temperature resistant plastic according to claim 1, characterized in that: The specific steps include: S1, mixing the graphene oxide composite carrier filler and the modified cerium dioxide nanofiller, adding them into an extruder for melt extrusion, granulating, controlling the melt extrusion temperature at 150-200° C., and obtaining a composite filler masterbatch; S2. Mix polyphenylene sulfide, the composite filler masterbatch described in step S1, dibutyl phthalate, and polytetrafluoroethylene at a mixing speed of 800-1000 rpm and a mixing time of 5-15 min. Extrude the mixture in an extruder to obtain a feed material at an extrusion temperature of 280-320° C. Then, the feed material is injection molded in an injection molding machine at an injection molding temperature of 300-320° C., an injection molding pressure of 100-200 MPa, and a holding time of 10-80 s to obtain a high temperature resistant plastic.
3. The method for preparing high temperature resistant plastic according to claim 2, characterized in that: In step S1, during the mixing process, the mixing speed is 1000-2000 rpm and the mixing time is 10-20 min.
4. The method for preparing high temperature resistant plastic according to claim 3, characterized in that: The method for preparing the graphene oxide composite carrier filler specifically comprises the following steps: (1) Add 0.3 g of graphene oxide to 25 mL of anhydrous ethanol, and disperse in a water bath for 30-60 min by ultrasonic dispersion. Transfer the suspension to a three-necked flask, and then add KH570 silane coupling agent. Pass nitrogen protection, and condense and reflux the reaction at 100-110 ° C for 10-12 h. The obtained mixed solution is filtered, and then rinsed with toluene solution, 70-80% ethanol solution, and deionized water for 3-5 times in sequence, each time using 50 mL. The obtained filter cake is freeze-dried at a freeze-drying temperature of -30 ° C to -50 ° C, and the freeze-drying time is 2-3 days to obtain KH570 modified graphene oxide; (2) Add the KH570 modified graphene oxide described in step (1) to the carboxyl-terminated nitrile rubber, stir for 3-5 min at 130-160° C. using a high-speed homogenizer, with a stirring speed of 10000-20000 rpm, and then cure at 80-90° C. for 1-2 h and at 100-120° C. for 2-3 h to obtain a graphene oxide composite carrier filler.
5. The method for preparing high temperature resistant plastic according to claim 4, characterized in that: In step (1), the amount of KH570 silane coupling agent added is 1.5-5 g.
6. The method for preparing high temperature resistant plastic according to claim 5, characterized in that: In step (2), the amount of carboxyl-terminated nitrile rubber added is 1-3 g.
7. The method for preparing high temperature resistant plastic according to claim 6, characterized in that: The preparation method of the modified cerium dioxide nanofiller specifically comprises the following steps: Dissolve 1-2 g of carboxymethyl chitosan in 60 mL of distilled water for standby use, prepare 100 mL of cerium nitrate hexahydrate solution with a mass fraction of 5-10%, then add the carboxymethyl chitosan solution to mix, control the temperature at 65-75 ° C, stir for 5-6 hours, after stirring, cool the reaction product to room temperature, centrifuge at a speed of 8000-10000 rpm, and centrifuge for 5-10 minutes. Remove the supernatant, wash the obtained precipitate with anhydrous ethanol and distilled water for 2-3 times, dry at a drying temperature of 50-60 ° C and a drying time of 8-12 hours, and then calcine at a calcination temperature of 500-600 ° C and a calcination time of 1-2 hours to obtain a modified cerium dioxide nanofiller.