A method for preparing ablation-resistant heat-insulating carbon aerogel composite material
Through nanorepair technology, the microstructure of carbon aerogel composite materials is optimized, and the performance weakening problem caused by shrinkage mismatch in traditional materials is solved, and the high ablation resistance and thermal insulation performance is improved, which is suitable for high-temperature applications.
Patent Information
- Application Number
- CN202410830366.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-06-25
AI Technical Summary
Due to the mismatch of the shrinkage of the fibers and the matrix, the microstructure of the material is uneven and its performance is weakened, making it difficult to meet the application of high ablation resistance and heat insulation requirements.
Using nanorepair method, ablation-resistant and heat-insulating carbon aerogel composite material is prepared by mixing phenolic resin, phenolic aerogel powder, dispersant and solvent. The method includes impregnation, aging, drying, carbonization and multiple nanorepair steps to optimize the microstructure of the material.
It significantly improves the ablation and oxidation resistance of the material, reduces density and thermal conductivity, and extends the stability of the material at high temperatures. It is suitable for high-temperature thermal protection systems.
Smart Images

Figure CN118637937B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of ablation-resistant composite materials, and in particular relates to a method for preparing ablation-resistant heat-insulating carbon aerogel composite materials. Background Art
[0002] Traditional C / C composite materials are widely used in various high-temperature thermal protection systems as excellent thermal protection materials due to their low density, small thermal expansion coefficient, high strength and modulus, good chemical stability and dimensional stability. However, higher service requirements have prompted researchers to change the traditional material design concept and continuously develop new thermal protection materials.
[0003] Traditional C / C composite materials are carbon fiber reinforced dense carbon matrix composite materials. By increasing the density of the matrix, the material's anti-ablation performance can be significantly improved, but the compact material structure will also lead to a decrease in thermal insulation performance, making its thermal conductivity higher. Therefore, this type of material is mostly used in service environments with low or even no requirements for thermal insulation.
[0004] As a new type of material, carbon aerogel combines the stability of carbon materials and the efficient thermal insulation properties of porous materials, and is an ideal ablation-resistant thermal insulation material. In addition, carbon aerogel has low strength and is usually combined with fibers to improve the mechanical properties of the material. However, the preparation of fiber-reinforced carbon aerogel composites is through carbonization by cracking of carbon sources. The shrinkage mismatch between the fibers and the matrix leads to an uneven microstructure of the material, and the performance is greatly weakened. Therefore, the development of a micro-nanostructure filling method is of vital importance to the development of traditional carbon aerogel composites.
[0005] In summary, it is very necessary to provide a method for preparing ablation-resistant and thermally insulating carbon aerogel composite materials. Summary of the invention
[0006] In order to solve one or more technical problems existing in existing carbon aerogel composite materials, the present invention provides a method for preparing an ablation-resistant and heat-insulating carbon aerogel composite material.
[0007] In a first aspect, the present invention provides a method for preparing an ablation-resistant and heat-insulating carbon aerogel composite material, the preparation method comprising the following steps:
[0008] (1) mixing a phenolic resin, a curing agent, a solvent and a dispersant uniformly to obtain a first phenolic solution, impregnating a fiber braid with the first phenolic solution, and then aging, drying and carbonizing the fiber braid in sequence to obtain a carbon aerogel composite material;
[0009] (2) mixing phenolic resin, phenolic aerogel powder, dispersant and solvent uniformly to obtain a second phenolic solution, impregnating the carbon aerogel composite material with the second phenolic solution and then standing, and then pre-carbonizing at 400-600° C. to obtain a pre-treated carbon aerogel composite material; the phenolic aerogel powder is obtained by aging, drying, grinding and sieving the first phenolic solution in sequence;
[0010] (3) mixing phenolic resin, curing agent, solvent and dispersant evenly to obtain a repair solution, impregnating the pretreated carbon aerogel composite material with the repair solution once, then performing ultrasonic treatment and secondary impregnation, and finally performing gelation, aging and carbonization in sequence;
[0011] (4) Repeating steps (2) and (3) 2 to 5 times in sequence to achieve nano-repair of the carbon aerogel composite material and obtain an ablation-resistant and heat-insulating carbon aerogel composite material.
[0012] Preferably, in step (1): the mass ratio of the phenolic resin, curing agent, solvent and dispersant is 20:(1-5):(80-120):(0-1); the curing agent is one or more of paraformaldehyde, hexamethylenetetramine, aniline, formaldehyde, melamine, carbonate, bicarbonate, alkali; the solvent is one or more of anhydrous ethanol, propanol, methanol, ethylene glycol; and / or the dispersant is one or more of deionized water, polyethylene glycol 400, polyethylene glycol 600 and polyethylene glycol 1000.
[0013] Preferably, in step (1): the impregnation is atmospheric pressure impregnation or vacuum impregnation, the pressure of the vacuum impregnation is 0.01-10 kPa; the impregnation time is 30-60 min; the aging is aging at 120-150° C. for 5-30 h; the drying is drying at 170-190° C. for 10-20 h; the carbonization is carried out under vacuum conditions or under inert gas protection; and / or the carbonization temperature is 600-1200° C., and the carbonization time is 1.5-3.5 h.
[0014] Preferably, in step (1): the fiber used in the fiber braided body is one or more of carbon fiber, quartz fiber, glass fiber, mullite fiber, phenolic fiber; and / or the structure of the fiber braided body is a needle-punched structure, a mesh structure, a 2.5D braided structure or a three-dimensional braided structure.
[0015] Preferably, in step (2): the mass ratio of the phenolic resin, phenolic aerogel powder, dispersant and solvent is 1:(0.1-1):(0.1-0.5):(5-10); the dispersant is one or more of triethylhexyl phosphoric acid, sodium dodecyl sulfate, methyl amyl alcohol, polyacrylamide; the solvent is one or more of anhydrous ethanol, propanol, methanol, ethylene glycol; and / or the particle size of the phenolic aerogel powder is 100-200 mesh.
[0016] Preferably, in step (2): the impregnation is performed at normal pressure; the impregnation time is 0.5 to 1 hour; and / or the standing time is 0.5 to 2 hours.
[0017] Preferably, in step (3): the mass ratio of the phenolic resin, curing agent, solvent and dispersant is 1:(0.1-0.5):(1-10):(0-1); the curing agent is one or more of paraformaldehyde, hexamethylenetetramine, aniline, formaldehyde, melamine, carbonate, bicarbonate, alkali; the solvent is one or more of anhydrous ethanol, propanol, methanol, ethylene glycol; and / or the dispersant is one or more of deionized water, polyethylene glycol 400, polyethylene glycol 600 and polyethylene glycol 1000.
[0018] Preferably, in step (3): the primary impregnation and / or the secondary impregnation is atmospheric pressure impregnation or vacuum impregnation, the pressure of the vacuum impregnation is 0.01-10 kPa; the time of the primary impregnation is 30-60 min; the time of the ultrasonic treatment is 15-30 min; and / or the time of the secondary impregnation is 10-30 min.
[0019] Preferably, in step (3): the gel is gelled at 80-100°C for 2-5 hours; the aging is aged at 150-180°C for 5-10 hours; the carbonization is carried out under vacuum conditions or under the protection of an inert gas; and / or the carbonization temperature is 600-1200°C, and the carbonization time is 1.5-3.5 hours.
[0020] In a second aspect, the present invention provides an ablation-resistant and heat-insulating carbon aerogel composite material prepared by the preparation method described in the first aspect of the present invention.
[0021] Compared with the prior art, the present invention has at least the following beneficial effects:
[0022] (1) The nano-repairing method used in the present invention for the carbon aerogel composite material when preparing the ablation-resistant and heat-insulating carbon aerogel composite material overcomes the problem of uneven microstructure caused by shrinkage mismatch in traditional carbon aerogel composite materials, and improves the ablation resistance and antioxidant properties of the material; the nano-repairing method in the present invention has a simple and efficient preparation process and is suitable for mass production.
[0023] (2) The ablation-resistant and heat-insulating carbon aerogel composite material obtained by the present invention has low density, good heat resistance and low ablation rate; the present invention combines a uniform carbon matrix with a fiber reinforcement, optimizes the microstructure of the carbon aerogel composite material, and designs and prepares an ablation-resistant and heat-insulating carbon aerogel composite material through the nano-repair method first proposed by the present invention, thereby broadening the application field of traditional C / C composite materials. The raw materials of the present invention are easily available, the reaction is simple and controllable, the preparation method is simple, the preparation cycle is short, and it is easy to industrialize. The mechanical strength of the ablation-resistant and heat-insulating carbon aerogel composite material obtained by the present invention is significantly improved; at the same time, the uniform micro-nano structure obtained after nano-repair can provide the material with good structural stability and excellent heat-insulating performance.
[0024] (3) The present invention greatly reduces the carbonization shrinkage of the carbon source, and at the same time, through process optimization, eliminates the time-consuming solvent replacement process, reduces the preparation cost, shortens the preparation cycle, and is suitable for mass production.
[0025] (4) Compared with existing materials, the density of the ablation-resistant and heat-insulating carbon aerogel composite material obtained by the present invention is 0.26-0.41 g / cm 3 ; The room temperature thermal conductivity is 0.055 to 0.068 W / (m·K); the residual weight after heating to 1000°C in an argon atmosphere is 94.5 to 97%; the residual weight after heating to 1000°C in an air atmosphere is 3 to 13%. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a scanning electron microscope image of the carbon aerogel composite material provided in Example 1 of the present invention;
[0027] Figure 2 This is a scanning electron microscope image of the ablation-resistant and heat-insulating carbon aerogel composite material provided in Example 1 of the present invention;
[0028] Figure 3 TG curve of the ablation-resistant and heat-insulating carbon aerogel composite material provided in Example 1 of the present invention under air atmosphere;
[0029] Figure 4 A compressive stress-strain curve diagram of the ablation-resistant and heat-insulating carbon aerogel composite material provided in Example 1 of the present invention;
[0030] Figure 5 The morphology comparison and surface temperature and back temperature curves of the ablation-resistant and heat-insulating carbon aerogel composite material provided in Example 1 of the present invention before and after butane ablation. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] In a first aspect, the present invention provides a method for preparing an ablation-resistant heat-insulating carbon aerogel composite material, the preparation method comprising the following steps:
[0033] (1) Phenolic resin, curing agent, solvent and dispersant are uniformly mixed to obtain a first phenolic solution, and a fiber braid is impregnated with the first phenolic solution, and then aged, dried and carbonized in sequence to obtain a carbon aerogel composite material; the present invention has no special requirements on the source of the phenolic resin, and a phenolic resin that can be directly purchased on the market can be used; in the present invention, the phenolic resin can be, for example, a boron phenolic resin; in the present invention, during the impregnation, the solution used for impregnation can completely cover the material to be impregnated; taking the impregnation of the fiber braid with the first phenolic solution as an example, during the impregnation, the amount of the first phenolic solution used can completely cover the fiber braid;
[0034] (2) mixing phenolic resin, phenolic aerogel powder, dispersant and solvent uniformly to obtain a second phenolic solution, impregnating the carbon aerogel composite material with the second phenolic solution and then standing, and then pre-carbonizing at 400-600°C to obtain a pre-treated carbon aerogel composite material; the phenolic aerogel powder is obtained by aging, drying, grinding and sieving the first phenolic solution in sequence; in step (2) of the present invention, the first phenolic solution used is the same as the first phenolic solution in step (1); in the present invention, the grinding is, for example, grinding by a mortar, and the sieving is, for example, sieving through a 100-200 mesh screen; in the present invention, the pre-carbonization time is, for example, 1-5 hours, and the rate of heating to the pre-carbonization temperature can be, for example, 4-10°C / min;
[0035] (3) Phenolic resin, curing agent, solvent and dispersant are mixed evenly to obtain a repair solution, and the pretreated carbon aerogel composite material is impregnated with the repair solution once, and then ultrasonic treatment and secondary impregnation are performed, and finally gelation, aging and carbonization are performed in sequence; in the present invention, this step is specifically: the pretreated carbon aerogel composite material is impregnated in the repair solution, first impregnated, then ultrasonicated, the ultrasonically treated material is not taken out, and atmospheric pressure impregnation or vacuum impregnation is continued. The material is not taken out during the whole process, and is directly treated in the repair solution. The role of ultrasonic treatment is to allow the repair solution to penetrate into the micro-nano pores that are difficult to enter. Impregnation after ultrasonic treatment can ensure that the material is fully impregnated. After the secondary impregnation is completed, the material is not taken out from the repair solution, but gelation, aging and carbonization are performed in situ;
[0036] (4) Repeating steps (2) and (3) 2 to 5 times in sequence to achieve nano-repair of the carbon aerogel composite material, and obtaining an ablation-resistant and heat-insulating carbon aerogel composite material; in the present invention, the carbon aerogel composite material obtained in step (1) shrinks and produces defects such as micro-nano gaps. The repair solution of the present invention introduces the precursor into the defects of the pretreated carbon aerogel composite material in the form of a solution, and then undergoes an in-situ sol-gel reaction to allow nanoparticles to be filled and compounded in the micro-nano gaps. Therefore, the repair in the present invention can be considered as nano-repair, and in fact, it can also be considered as a micro-nano filling treatment.
[0037] The nano-repair method used by the present invention for the carbon aerogel composite material when preparing the ablation-resistant and heat-insulating carbon aerogel composite material is different from the method of multiple impregnations with the same impregnation liquid in the prior art. This impregnation method in the prior art is usually mainly for achieving material densification, but is not suitable for repairing defects such as micro-nano gaps in the carbon aerogel composite material, because this method will destroy the porous structure of the aerogel material. The present invention optimizes the microstructure (micro-nanostructure) of traditional carbon fiber reinforced carbon aerogel through original nano-repair. The present invention first introduces phenolic aerogel powder into a second phenolic solution to impregnate the carbon aerogel composite material, and then pre-carbonizes it at 400-600°C to obtain a pre-treated carbon aerogel composite material. Such a pre-treatment operation can effectively improve the wettability between the inorganic carbon aerogel composite material and the organic repair solution, which is beneficial to improve the repair effect of the repair solution on the carbon aerogel composite material, and obtain a more excellent ablation-resistant and heat-insulating carbon aerogel composite material; this is because the carbon aerogel composite material is an inorganic material after carbonization treatment, and the phenolic resin in the repair solution is an organic material, and the compatibility (wettability) between the two is relatively poor. The present invention first introduces the phenolic aerogel powder uniformly into the carbon aerogel skeleton in the form of a solution, and then pre-carbonizes it at a temperature of 400-600°C. The invention discloses a method for pre-carbonizing the phenolic resin by pre-carbonizing the phenolic resin at a temperature of 100 to 600°C (the phenolic resin can be completely converted into an inorganic material only at a temperature greater than 600°C), that is, the phenolic resin is pre-carbonized and is in a state of being both an organic material and an inorganic material, thus playing a role of a bridge. On the one hand, it has a good combination with the carbon aerogel composite material, and on the other hand, it has a good combination with the subsequently introduced organic repair solution, thereby promoting the combination and wetting of the organic material and the inorganic material. The invention finds that if the phenolic aerogel powder is not added to the second phenolic solution, the second phenolic solution will tightly wrap the carbon aerogel composite material to be repaired, which is not conducive to the immersion of the repair solution. In addition, the coating layer will form a dense layer on the skeleton of the carbon aerogel composite material, and the in-situ aerogel generated by the reaction of the repair solution will grow on the dense layer. There will be an isolation layer between the aerogel generated by the repair solution and the original aerogel, which will greatly affect the structure and performance of the material.
[0038] The nano-repairing method used by the present invention for the carbon aerogel composite material in the preparation of the ablation-resistant heat-insulating carbon aerogel composite material overcomes the problem of uneven microstructure caused by shrinkage mismatch of the traditional carbon aerogel composite material, and improves the ablation resistance and oxidation resistance of the material; the nano-repairing method in the present invention has a simple preparation process, high efficiency, and is suitable for mass production. The ablation-resistant heat-insulating carbon aerogel composite material obtained by the present invention has low density, good heat resistance, and low ablation rate; the present invention combines a uniform carbon matrix with a fiber reinforcement, and optimizes the microstructure of the carbon aerogel composite material. The nano-repairing method first proposed by the present invention designs and prepares an ablation-resistant heat-insulating carbon aerogel composite material, broadens the application field of traditional C / C composite materials, and the raw materials of the present invention are easy to obtain, the reaction is simple and controllable, the preparation method is simple, the preparation cycle is short, and it is easy to industrialize. The mechanical strength of the ablation-resistant heat-insulating carbon aerogel composite material obtained by the present invention is significantly improved; at the same time, the uniform micro-nano structure obtained after nano-repair can provide the material with good structural stability and excellent heat insulation performance. Compared with existing materials, the density of the ablation-resistant heat-insulating carbon aerogel composite material obtained by the present invention is 0.26-0.41 g / cm 3 ; The room temperature thermal conductivity is 0.055 to 0.068 W / (m·K); the residual weight after heating to 1000°C in an argon atmosphere is 94.5 to 97%, preferably 95.5 to 96.5%; the residual weight after heating to 1000°C in an air atmosphere is 3 to 13%, preferably 9.9 to 12.6% (the residual weight of the carbon aerogel composite material in the prior art after heating to 1000°C in an air atmosphere is usually 0%).
[0039] According to some preferred embodiments, in step (1): the mass ratio of the phenolic resin, curing agent, solvent and dispersant is 20:(1-5):(80-120):(0-1). The present invention finds that if the curing agent is too little, the resin cannot be cured and formed, and if it is too much, the degree of curing is too high and the aerogel structure cannot be formed; if the amount of solvent is too little, the role of the solvent in synthesizing aerogel cannot be played, and if it is too much, the strength of the aerogel is too low and cannot be formed, and the present invention preferably adds an appropriate amount of dispersant to help the uniform dispersion of the resin in the solution; the curing agent is one or more of paraformaldehyde, hexamethylenetetramine, aniline, formaldehyde, melamine, carbonate, bicarbonate, and alkali; the solvent is one or more of anhydrous ethanol, propanol, methanol, and ethylene glycol; and / or the dispersant is one or more of deionized water, polyethylene glycol 400, polyethylene glycol 600, and polyethylene glycol 1000.
[0040] According to some preferred embodiments, in step (1): the impregnation is atmospheric pressure impregnation or vacuum impregnation, and the pressure (absolute pressure) of the vacuum impregnation is 0.01-10 kPa; in the present invention, the pressure of the atmospheric pressure impregnation is, for example, 101.3 kPa; the impregnation time is 30-60 min (for example, 30, 35, 40, 45, 50, 55 or 60 min); the aging is aging at 120-150° C. (for example, 120° C., 125° C., 130° C., 140° C., 145° C. or 150° C.) for 5-30 h (for example, 5, 10, 15, 20, 25 or 30 h); the drying is drying at 170-190° C. (for example, 170° C., 175° C., 180° C., 185° C. or 190° C.) for 10-20 h (for example, 10, 12, 15, 1 8 or 20h); the carbonization is carried out under vacuum conditions or under the protection of an inert gas; and / or the carbonization temperature is 600-1200°C (for example, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C or 1200°C), preferably, the carbonization temperature is 650-1200°C, and the carbonization time is 1.5-3.5h (for example, 1.5, 2, 2.5, 3 or 3.5h); in the present invention, when carbonizing, for example, the material to be carbonized is first placed in a carbonization furnace, and after sealing, the vacuum is continuously drawn for 15-30min, and then the inert gas is continuously introduced for 10-20min, and then the temperature is raised to 600-1200°C for carbonization treatment; wherein the inert gas is, for example, argon or nitrogen, and the heating rate is, for example, 4-10°C / min.
[0041] According to some preferred embodiments, in step (1): the fibers used in the fiber braided body include but are not limited to carbon fiber, quartz fiber, glass fiber, mullite fiber, phenolic fiber, etc., preferably, the fibers used in the fiber braided body are one or more of carbon fiber, quartz fiber, glass fiber, mullite fiber, phenolic fiber; and / or the selected fiber braided body structure includes but is not limited to continuous fiber needle punched structure, mesh structure, 2.5D braided structure or three-dimensional braided structure, preferably, the structure of the fiber braided body is needle punched structure, mesh structure, 2.5D braided structure or three-dimensional braided structure.
[0042] According to some specific implementation methods, step (1) is: phenolic resin, curing agent, solvent and dispersant are mixed uniformly in proportion to obtain a first phenolic solution, a fiber braid is placed in the first phenolic solution for normal pressure impregnation or vacuum impregnation for 30 to 60 minutes, and aged at 120 to 150°C for 5 to 30 hours; after cooling, the fiber braid is taken out, dried at 170 to 190°C for 10 to 20 hours, and then heated to 600 to 1200°C in vacuum or under the protection of inert gas and kept warm for 1.5 to 3.5 hours to obtain a carbon aerogel composite material; in the present invention, preferably In-situ aging in the first phenolic solution is selected, that is, after impregnation, the impregnated fiber braid is directly placed in the first phenolic solution for in-situ aging at 120-150°C for 5-30 hours. The present invention finds that during the aging process, the solution gradually becomes solid, and at the same time, the solidification of the resin will produce a large amount of gas to form holes in the material, so that the original solution (the first phenolic solution) can play a role in filling the holes. If the fiber braid is taken out of the first phenolic solution after impregnation, it will cause the internal solution to sink due to gravity, resulting in uneven internal phenolic content.
[0043] According to some preferred embodiments, in step (2): the mass ratio of the phenolic resin, phenolic aerogel powder, dispersant and solvent is 1: (0.1-1): (0.1-0.5): (5-10); in the present invention, preferably, in the second phenolic solution, the mass ratio of the phenolic resin, phenolic aerogel powder, dispersant and solvent is 1: (0.1-1): (0.1-0.5): (5-10). The present invention finds that if the phenolic aerogel powder is too little, it will not be able to play a sufficient bridging role on the material skeleton, which will make the phenolic aerogel powder dispersed more sparsely, and some positions will be exposed, and if the phenolic aerogel powder is too much, agglomeration will occur. This will affect the performance of the material; the dispersant is one or more of triethylhexyl phosphoric acid, sodium dodecyl sulfate, methyl amyl alcohol, and polyacrylamide; in the second phenolic solution of the present invention, the dispersant is preferably one or more of triethylhexyl phosphoric acid, sodium dodecyl sulfate, methyl amyl alcohol, and polyacrylamide, so that the phenolic aerogel powder can be evenly dispersed in the second phenolic solution to avoid agglomeration, which is beneficial to ensure that the wettability between the inorganic material carbon aerogel composite material and the organic repair solution is effectively improved; the solvent is one or more of anhydrous ethanol, propanol, methanol, and ethylene glycol; and / or the particle size of the phenolic aerogel powder is 100 to 200 meshes.
[0044] According to some preferred embodiments, in step (2): the impregnation is atmospheric pressure impregnation; the impregnation time is 0.5 to 1 hour; and / or the standing time is 0.5 to 2 hours.
[0045] According to some specific implementation methods, step (2) is: first prepare a second phenolic solution, then put the carbon aerogel composite material into the second phenolic solution and immerse it for 0.5 to 1 hour, then take it out, let it stand for 0.5 to 2 hours, and then pre-carbonize it in a carbonization furnace at 400 to 600°C; in the present invention, preferably, after immersion and before pre-carbonization, let it stand for 0.5 to 2 hours. In this way, since the purpose of step (2) is to evenly form a layer of inorganic-organic bridges on the aerogel skeleton, due to the immersion effect, there will also be a large amount of second phenolic solution in the pores of the aerogel. By letting it stand for 0.5 to 2 hours, it is free to discharge due to gravity, which is beneficial to retaining the original structure of the aerogel and also beneficial to the immersion of the repair solution.
[0046] According to some preferred embodiments, in step (3): the mass ratio of the phenolic resin, curing agent, solvent and dispersant is 1:(0.1-0.5):(1-10):(0-1); when the pretreated carbon aerogel composite material is impregnated with the repair solution in step (3), since the generated aerogel is generated on the original material skeleton, its synthesis is easier than step (1). Therefore, in the repair solution of step (3), the mass ratio of the phenolic resin, curing agent, solvent and dispersant is appropriately adjusted to 1:(0.1-0.5):(1-10):(0-1), which is beneficial to promote the production of aerogel and shorten the repair cycle; the curing agent is one or more of paraformaldehyde, hexamethylenetetramine, aniline, formaldehyde, melamine, carbonate, bicarbonate, alkali; the solvent is one or more of anhydrous ethanol, propanol, methanol, ethylene glycol; and / or the dispersant is one or more of deionized water, polyethylene glycol 400, polyethylene glycol 600 and polyethylene glycol 1000.
[0047] According to some preferred embodiments, in step (3): the primary impregnation and / or the secondary impregnation is atmospheric pressure impregnation or vacuum impregnation, the pressure of the vacuum impregnation is 0.01 to 10 kPa; the time of the primary impregnation is 30 to 60 min; the time of the ultrasonic treatment is 15 to 30 min; and / or the time of the secondary impregnation is 10 to 30 min.
[0048] According to some preferred embodiments, in step (3): the gel is gelled at 80-100°C (e.g., 80°C, 90°C, or 100°C) for 2-5h (e.g., 2, 2.5, 3, 3.5, 4, 4.5, or 5h); the aging is aging at 150-180°C (e.g., 150°C, 160°C, 170°C, or 180°C) for 5-10h (e.g., 5, 6, 7, 8, 9, or 10h); The carbonization is carried out under vacuum conditions or under inert gas protection; and / or the carbonization temperature is 600-1200°C (for example, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C or 1200°C), preferably, the carbonization temperature is 650-1200°C, and the carbonization time is 1.5-3.5h (for example, 1.5, 2, 2.5, 3 or 3.5h).
[0049] According to some specific implementation methods, step (3) is: preparing a repair solution, mixing phenolic resin, curing agent, solvent and dispersant in proportion to obtain a repair solution; placing the pretreated carbon aerogel composite material into the repair solution for normal pressure impregnation or vacuum impregnation (primary impregnation) for 30 to 60 minutes, then ultrasonically treating for 15 to 30 minutes, and impregnating again (secondary impregnation) for 15 to 30 minutes, and then heating at 80 to 100° C. for 2 to 5 hours to form a gel, and then aging at 150 to 180° C. for 5 to 10 hours, and then carbonizing.
[0050] According to some preferred embodiments, in the process of repeating step (2) and step (3) 2 to 5 times, the repair solutions used are the same or different; preferably, in the process of repeating step (2) and step (3) 2 to 5 times, the sum of the mass percentages of phenolic resin and curing agent contained in the repair solution used in the latter nano-repair is not greater than the mass percentages of phenolic resin and curing agent contained in the repair solution used in the previous nano-repair, for example, by increasing the amount of solvent added, the solid content of the repair solution is made lower, which is more conducive to the immersion of the repair solution; in the present invention, repeating step (2) and step (3) once can be recorded as one nano-repair.
[0051] In a second aspect, the present invention provides an ablation-resistant and heat-insulating carbon aerogel composite material prepared by the preparation method described in the first aspect of the present invention.
[0052] The present invention will be further described below by way of examples, but the protection scope of the present invention is not limited to these embodiments.
[0053] Example 1
[0054] ① Preparation of carbon aerogel composite materials: Phenolic resin (phenolic resin THC-400), hexamethylenetetramine, ethylene glycol and deionized water were mixed uniformly in a mass ratio of 20:1.5:90:0.1 to obtain a first phenolic solution, and then a carbon fiber braid (three-dimensional braided structure) was placed in the first phenolic solution for impregnation at normal pressure for 60 minutes (impregnation temperature was 25°C), and aged at 150°C for 10 hours; after cooling to 25°C, the impregnated carbon fiber braid was taken out, dried at 180°C for 15 hours, and then heated to 800°C under argon gas protection and carbonized for 2 hours at a heating rate of 5°C / min to obtain a carbon aerogel composite material.
[0055] ② First, prepare a second phenolic solution, mix phenolic resin (phenolic resin THC-400), phenolic aerogel powder, sodium dodecyl sulfate and anhydrous ethanol in a mass ratio of 1:0.1:0.5:10 to obtain a second phenolic solution, then put the carbon aerogel composite material into the second phenolic solution for atmospheric impregnation for 1 hour (the impregnation temperature is 25°C), take it out, stand it at room temperature for 1 hour, and then pre-carbonize it in a 400°C carbonization furnace under argon gas protection for 2 hours (the heating rate to 400°C is 25°C). The phenolic aerogel powder is prepared by mixing phenolic resin (phenolic resin THC-400), hexamethylenetetramine, ethylene glycol and deionized water in a mass ratio of 20:1.5:90:0.1 to obtain a first phenolic solution, then aging the first phenolic solution at 150°C for 10 hours, and then drying at 180°C for 15 hours, and finally grinding and sieving with a mortar to obtain a phenolic aerogel powder with a particle size of 100 to 200 meshes.
[0056] ③ Prepare a repair solution, mix phenolic resin (phenolic resin THC-400), sodium carbonate, ethylene glycol and polyethylene glycol 400 in a mass ratio of 1:0.1:5:0.5 to obtain a repair solution; place the pretreated carbon aerogel composite material into the repair solution for vacuum impregnation for 30 minutes (the vacuum impregnation temperature is 25°C and the pressure is 5 kPa), then ultrasonically treat for 15 minutes, and then impregnate at normal pressure for 20 minutes (the normal pressure impregnation temperature is 25°C), then heat at 80°C for 5 hours to form a gel, then age at 180°C for 5 hours, and then heat to 800°C under argon gas protection and carbonize for 2 hours at a heating rate of 5°C / min to achieve a one-time nano-repair of the carbon aerogel composite material.
[0057] ④ Repeat step ② and step ③ twice in sequence to realize secondary nano-repair of the carbon aerogel composite material and tertiary nano-repair of the carbon aerogel composite material in sequence, and obtain ablation-resistant and heat-insulating carbon aerogel composite material; in the secondary nano-repair and tertiary nano-repair, other operations are consistent with the primary nano-repair, except that, in the secondary nano-repair and tertiary nano-repair, the preparation of the repair solution is: phenolic resin (phenolic resin THC-400), sodium carbonate, ethylene glycol and polyethylene glycol 400 are evenly mixed in a mass ratio of 1:0.1:7:0.1 to obtain a repair solution.
[0058] The density of the ablation-resistant heat-insulating carbon aerogel composite material prepared in this embodiment was measured to be 0.36 g / cm 3 .
[0059] The room temperature thermal conductivity of the ablation-resistant and heat-insulating carbon aerogel composite material prepared in this embodiment was tested according to the standard "GB / T 3139-2005 Test method for thermal conductivity of fiber-reinforced plastics", and the room temperature thermal conductivity was found to be 0.058 W / m·K.
[0060] According to the standard "GB / T 1448-2005 Test method for compression properties of fiber reinforced plastics", the longitudinal compressive strength (longitudinal compressive strength under 5% compression deformation) of the ablation-resistant and heat-insulating carbon aerogel composite material prepared in this embodiment is 2.13 MPa. The results are shown in Table 1.
[0061] It was measured that the residual weight of the ablation-resistant and heat-insulating carbon aerogel composite material prepared in this embodiment after being heated to 1000° C. in an argon atmosphere was 95.8%; and the residual weight after being heated to 1000° C. in an air atmosphere was 10.3%.
[0062] The morphology comparison and the surface temperature and back temperature curves of the ablation-resistant heat-insulating carbon aerogel composite material provided in Example 1 of the present invention before and after butane ablation are shown in FIG. Figure 5 As shown, from Figure 5 As can be seen from (a) and (b), only a small amount of oxidation occurs on the surface of the material after ablation, and the surface morphology has hardly changed. In the butane ablation test of the ablation-resistant and heat-insulating carbon aerogel composite material in this embodiment, the surface temperature is 1100°C, and after the test time is 600s, the back temperature is measured to be 203.9°C.
[0063] Example 2
[0064] ① Preparation of carbon aerogel composite materials: Phenolic resin (phenolic resin THC-800), polyformaldehyde, ethylene glycol and polyethylene glycol 400 are mixed uniformly in a mass ratio of 20:1:120:0.5 to obtain a first phenolic solution, and then a quartz fiber braid (three-dimensional braided structure) is placed in the first phenolic solution for vacuum impregnation for 30 minutes (vacuum impregnation temperature is 25°C, pressure is 5kPa), and aged at 120°C for 30 hours; after cooling to 25°C, the impregnated quartz fiber braid is taken out, dried at 190°C for 10 hours, and then heated to 1000°C under argon gas protection and carbonized for 1.5 hours at a heating rate of 10°C / min to obtain a carbon aerogel composite material.
[0065] ② First, prepare a second phenolic solution, mix phenolic resin (phenolic resin THC-800), phenolic aerogel powder, triethylhexyl phosphoric acid and methanol in a mass ratio of 1:0.1:0.5:10 to obtain a second phenolic solution, then put the carbon aerogel composite material into the second phenolic solution for atmospheric impregnation for 0.5 h (the impregnation temperature is 25 ° C), then take it out, stand it at room temperature 25 ° C for 0.5 h, and then pre-carbonize it in a 400 ° C carbonization furnace under argon gas protection for 5 h (the heating rate of heating to 400 ° C is 25 ° C). The rate is 10℃ / min to obtain a pretreated carbon aerogel composite material, wherein the phenolic aerogel powder is prepared by mixing phenolic resin (phenolic resin THC-800), paraformaldehyde, ethylene glycol and polyethylene glycol 400 in a mass ratio of 20:1:120:0.5 to obtain a first phenolic solution, then aging the first phenolic solution at 120℃ for 30h, and then drying it at 190℃ for 10h, and finally grinding and sieving it with a mortar to obtain a phenolic aerogel powder with a particle size of 100-200 mesh.
[0066] ③ Prepare the repair solution, mix phenolic resin (phenolic resin THC-800), formaldehyde and anhydrous ethanol in a mass ratio of 1:0.5:3 to obtain a repair solution; put the pretreated carbon aerogel composite material into the repair solution for atmospheric pressure impregnation for 60 minutes (the atmospheric pressure impregnation temperature is 25°C), then ultrasonically treat for 15 minutes, and then vacuum impregnate for 20 minutes (the vacuum impregnation temperature is 25°C and the pressure is 5kPa), then heat at 80°C for 3 hours to form a gel, then age at 150°C for 10 hours, and then heat to 800°C under argon gas protection and carbonize for 2 hours at a heating rate of 10°C / min to achieve a one-time nano-repair of the carbon aerogel composite material.
[0067] ④ Repeat steps ② and ③ three times in sequence to successively implement secondary nano-repair of the carbon aerogel composite material, tertiary nano-repair of the carbon aerogel composite material and quadruple nano-repair of the carbon aerogel composite material to obtain ablation-resistant and heat-insulating carbon aerogel composite material; in the secondary nano-repair, the other operations are consistent with the primary nano-repair, except that, in the secondary nano-repair, the preparation of the repair solution is as follows: phenolic resin (phenolic resin THC-800), formaldehyde and anhydrous ethanol are mixed in a mass ratio of 1:0.5:5 to obtain a repair solution; in the tertiary nano-repair and the quadruple nano-repair, the other operations are consistent with the primary nano-repair, except that, in the tertiary nano-repair and the quadruple nano-repair, the preparation of the repair solution is as follows: phenolic resin (phenolic resin THC-800), formaldehyde and anhydrous ethanol are mixed in a mass ratio of 1:0.5:7 to obtain a repair solution.
[0068] Example 3
[0069] ① Preparation of carbon aerogel composite materials: Phenolic resin (phenolic resin THC-400), aniline, methanol and polyethylene glycol 400 are mixed uniformly in a mass ratio of 20:5:80:0.5 to obtain a first phenolic solution, and then a glass fiber braid (three-dimensional braided structure) is placed in the first phenolic solution for atmospheric impregnation for 60 minutes (the atmospheric impregnation temperature is 25°C), and aged at 130°C for 20 hours; after cooling to 25°C, the impregnated glass fiber braid is taken out, dried at 170°C for 20 hours, and then heated to 1200°C under nitrogen gas protection and carbonized for 2 hours at a heating rate of 4°C / min to obtain a carbon aerogel composite material.
[0070] ② First, prepare a second phenolic solution, mix phenolic resin (phenolic resin THC-400), phenolic aerogel powder, triethylhexyl phosphoric acid and propanol in a mass ratio of 1:0.1:0.5:8 to obtain a second phenolic solution, then put the carbon aerogel composite material into the second phenolic solution for atmospheric impregnation for 1 hour (the impregnation temperature is 25°C) and then take it out, stand it at room temperature at 25°C for 2 hours, and then pre-carbonize it in a 600°C carbonization furnace under nitrogen gas protection for 1.5 hours (the heating rate to 600°C is 25°C). The pretreated carbon aerogel composite material is obtained by mixing phenolic resin (phenolic resin THC-400), aniline, methanol and polyethylene glycol 400 in a mass ratio of 20:5:80:0.5 to obtain a first phenolic solution, then aging the first phenolic solution at 130°C for 20h, and then drying it at 170°C for 20h, and finally grinding and sieving it in a mortar to obtain a phenolic aerogel powder with a particle size of 100 to 200 meshes.
[0071] ③ Prepare the repair solution: mix phenolic resin (phenolic resin THC-400), formaldehyde, methanol and deionized water in a mass ratio of 1:0.5:3:0.5 to obtain a repair solution; place the pretreated carbon aerogel composite material into the repair solution for vacuum impregnation for 60 minutes (the vacuum impregnation temperature is 25°C and the pressure is 1 kPa), then ultrasonically treat for 20 minutes, and then vacuum impregnate for 10 minutes (the vacuum impregnation temperature is 25°C and the pressure is 2 kPa), then heat at 80°C for 3 hours to form a gel, then age at 180°C for 5 hours, and then heat to 650°C under nitrogen gas protection and carbonize for 3.5 hours at a heating rate of 5°C / min to achieve a one-time nano-repair of the carbon aerogel composite material.
[0072] ④ Repeat steps ② and ③ four times in sequence to successively implement secondary nano-repair of the carbon aerogel composite material, tertiary nano-repair of the carbon aerogel composite material, fourth nano-repair of the carbon aerogel composite material and fifth nano-repair of the carbon aerogel composite material to obtain ablation-resistant and heat-insulating carbon aerogel composite material; in the secondary nano-repair and tertiary nano-repair, the other operations are consistent with the primary nano-repair, except that, in the secondary nano-repair and tertiary nano-repair, the preparation of the repair solution is as follows: phenolic resin (phenolic resin THC-400), formaldehyde, methanol, and deionized water are mixed in a mass ratio of 1:0.5:5:0.5 to obtain a repair solution; in the fourth nano-repair and fifth nano-repair, the other operations are consistent with the primary nano-repair, except that, in the fourth nano-repair and fifth nano-repair, the preparation of the repair solution is as follows: phenolic resin (phenolic resin THC-400), formaldehyde, methanol, and deionized water are mixed in a mass ratio of 1:0.5:10:0.5 to obtain a repair solution.
[0073] Example 4
[0074] Embodiment 4 is substantially the same as Embodiment 1, except that:
[0075] ④ Repeat step ② and step ③ twice in sequence to achieve secondary nano-repair of the carbon aerogel composite material and tertiary nano-repair of the carbon aerogel composite material in sequence to obtain ablation-resistant and heat-insulating carbon aerogel composite material; in the secondary nano-repair and tertiary nano-repair, the preparation of the repair solution is: phenolic resin (phenolic resin THC-400), sodium carbonate, ethylene glycol and polyethylene glycol 400 are uniformly mixed in a mass ratio of 1:0.1:5:0.5 to obtain a repair solution.
[0076] Example 5
[0077] Example 5 is substantially the same as Example 1, except that:
[0078] ② First, prepare a second phenolic solution, mix phenolic resin (phenolic resin THC-400), phenolic aerogel powder, sodium dodecyl sulfate and anhydrous ethanol in a mass ratio of 1:0.05:0.5:10 to obtain a second phenolic solution, then put the carbon aerogel composite material into the second phenolic solution for atmospheric impregnation for 1 hour (the impregnation temperature is 25°C) and then take it out, stand it at room temperature for 1 hour, and then pre-carbonize it in a 400°C carbonization furnace under argon gas protection for 2 hours (the heating rate of heating to 400°C is 25°C). The pretreated carbon aerogel composite material is obtained by mixing phenolic resin (phenolic resin THC-400), hexamethylenetetramine, ethylene glycol and deionized water in a mass ratio of 20:1.5:90:0.1 to obtain a first phenolic solution, then aging the first phenolic solution at 150°C for 10 hours, and then drying it at 180°C for 15 hours. Finally, grinding and sieving with a mortar to obtain a phenolic aerogel powder with a particle size of 100 to 200 meshes.
[0079] Example 6
[0080] Embodiment 6 is substantially the same as Embodiment 1, except that:
[0081] ② First, prepare a second phenolic solution, mix phenolic resin (phenolic resin THC-400), phenolic aerogel powder, sodium dodecyl sulfate and anhydrous ethanol in a mass ratio of 1:2:0.5:10 to obtain a second phenolic solution, then put the carbon aerogel composite material into the second phenolic solution for atmospheric impregnation for 1 hour (the impregnation temperature is 25°C) and then take it out, stand it at room temperature for 1 hour, and then pre-carbonize it in a carbonization furnace at 400°C for 2 hours under argon gas protection (the heating rate to 400°C is 5℃ / min), and a pretreated carbon aerogel composite material is obtained, wherein the phenolic aerogel powder is prepared by: mixing phenolic resin (phenolic resin THC-400), hexamethylenetetramine, ethylene glycol and deionized water in a mass ratio of 20:1.5:90:0.1 to obtain a first phenolic solution, then aging the first phenolic solution at 150℃ for 10h, and then drying at 180℃ for 15h, and finally grinding and sieving with a mortar to obtain a phenolic aerogel powder with a particle size of 100-200 mesh.
[0082] Example 7
[0083] Example 7 is substantially the same as Example 1, except that:
[0084] ③ Prepare a repair solution, mix phenolic resin (phenolic resin THC-400), sodium carbonate, ethylene glycol and polyethylene glycol 400 in a mass ratio of 20:1.5:90:0.1 to obtain a repair solution; place the pretreated carbon aerogel composite material into the repair solution for vacuum impregnation for 30 minutes (the vacuum impregnation temperature is 25°C and the pressure is 5 kPa), then ultrasonically treat for 15 minutes, and then impregnate at normal pressure for 20 minutes (the normal pressure impregnation temperature is 25°C), then heat at 80°C for 5 hours to form a gel, then age at 180°C for 5 hours, and then heat to 800°C under argon gas protection and carbonize for 2 hours at a heating rate of 5°C / min to achieve a one-time nano-repair of the carbon aerogel composite material.
[0085] ④ Repeat step ② and step ③ twice in sequence to achieve secondary nano-repair of the carbon aerogel composite material and tertiary nano-repair of the carbon aerogel composite material in sequence to obtain ablation-resistant and heat-insulating carbon aerogel composite material; in the secondary nano-repair and tertiary nano-repair, the preparation of the repair solution is: phenolic resin (phenolic resin THC-400), sodium carbonate, ethylene glycol and polyethylene glycol 400 are mixed uniformly in a mass ratio of 20:1.5:90:0.1 to obtain a repair solution.
[0086] Comparative Example 1
[0087] ① Preparation of carbon aerogel composite materials: Phenolic resin (phenolic resin THC-400), hexamethylenetetramine, ethylene glycol and deionized water were mixed uniformly in a mass ratio of 20:1.5:90:0.1 to obtain a first phenolic solution, and then a carbon fiber braid (three-dimensional braided structure) was placed in the first phenolic solution for impregnation at normal pressure for 60 minutes (impregnation temperature was 25°C), and aged at 150°C for 10 hours; after cooling to 25°C, the impregnated carbon fiber braid was taken out, dried at 180°C for 15 hours, and then heated to 800°C under argon gas protection and carbonized for 2 hours at a heating rate of 5°C / min to obtain a carbon aerogel composite material.
[0088] ② Prepare a repair solution, mix phenolic resin (phenolic resin THC-400), sodium carbonate, ethylene glycol and polyethylene glycol 400 in a mass ratio of 1:0.1:5:0.5 to obtain a repair solution; place the carbon aerogel composite material in the repair solution for vacuum impregnation for 30 minutes (the vacuum impregnation temperature is 25°C and the pressure is 5 kPa), then ultrasonically treat for 15 minutes, and then impregnate at normal pressure for 20 minutes (the normal pressure impregnation temperature is 25°C), then heat at 80°C for 5 hours to form a gel, then age at 180°C for 5 hours, and then heat to 800°C under argon gas protection and carbonize for 2 hours at a heating rate of 5°C / min to achieve one-time repair of the carbon aerogel composite material.
[0089] ③ Repeat step ② twice in sequence to achieve secondary repair of the carbon aerogel composite material and tertiary repair of the carbon aerogel composite material in sequence, to obtain ablation-resistant and heat-insulating carbon aerogel composite material; in the secondary repair and tertiary repair, other operations are consistent with the primary repair, the difference is that, in the secondary repair and tertiary repair, the preparation of the repair solution is: phenolic resin (phenolic resin THC-400), sodium carbonate, ethylene glycol and polyethylene glycol 400 are mixed uniformly in a mass ratio of 1:0.1:7:0.1 to obtain a repair solution.
[0090] Comparative Example 2
[0091] Comparative Example 2 is substantially the same as Example 1, except that:
[0092] ② First, prepare a second phenolic solution, mix phenolic resin (phenolic resin THC-400) and anhydrous ethanol in a mass ratio of 1:10 to obtain a second phenolic solution, and then put the carbon aerogel composite material into the second phenolic solution for impregnation at normal pressure for 1 hour (the impregnation temperature is 25°C), then take it out, let it stand at room temperature for 1 hour, and then pre-carbonize it in a 400°C carbonization furnace under argon gas protection for 2 hours (the heating rate to 400°C is 5°C / min) to obtain a pretreated carbon aerogel composite material.
[0093] Comparative Example 3
[0094] Comparative Example 3 is substantially the same as Example 1, except that:
[0095] ② First, prepare a second phenolic solution, mix phenolic resin (phenolic resin THC-400), phenolic aerogel powder, sodium dodecyl sulfate and anhydrous ethanol in a mass ratio of 1:0.1:0.5:10 to obtain a second phenolic solution, then put the carbon aerogel composite material into the second phenolic solution for atmospheric impregnation for 1 hour (the impregnation temperature is 25°C), take it out, stand it at room temperature for 1 hour, and then carbonize it in a carbonization furnace at 800°C for 2 hours (the heating rate to 800°C is 25°C) under argon gas protection. The phenolic aerogel powder is prepared by mixing phenolic resin (phenolic resin THC-400), hexamethylenetetramine, ethylene glycol and deionized water in a mass ratio of 20:1.5:90:0.1 to obtain a first phenolic solution, then aging the first phenolic solution at 150°C for 10 hours, and then drying at 180°C for 15 hours, and finally grinding and sieving with a mortar to obtain a phenolic aerogel powder with a particle size of 100 to 200 meshes.
[0096] Comparative Example 4
[0097] ① Preparation of carbon aerogel composite materials: Phenolic resin (phenolic resin THC-400), hexamethylenetetramine, ethylene glycol and deionized water were mixed uniformly in a mass ratio of 20:1.5:90:0.1 to obtain a first phenolic solution, and then a carbon fiber braid (three-dimensional braided structure) was placed in the first phenolic solution for impregnation at normal pressure for 60 minutes (impregnation temperature was 25°C), and aged at 150°C for 10 hours; after cooling to 25°C, the impregnated carbon fiber braid was taken out, dried at 180°C for 15 hours, and then heated to 800°C under argon gas protection and carbonized for 2 hours at a heating rate of 5°C / min to obtain a carbon aerogel composite material.
[0098] ② Prepare the repair solution, mix phenolic resin (phenolic resin THC-400), hexamethylenetetramine, ethylene glycol and deionized water in a mass ratio of 20:1.5:90:0.1 to obtain a repair solution; place the carbon aerogel composite material in the repair solution for vacuum impregnation for 30 minutes (the vacuum impregnation temperature is 25°C and the pressure is 5 kPa), then ultrasonically treat for 15 minutes, and then impregnate at normal pressure for 20 minutes (the normal pressure impregnation temperature is 25°C), then heat at 80°C for 5 hours to form a gel, then age at 180°C for 5 hours, and then heat to 800°C under argon gas protection and carbonize for 2 hours at a heating rate of 5°C / min to achieve one-time repair of the carbon aerogel composite material.
[0099] ③ Repeat step ② twice in sequence to achieve secondary repair of the carbon aerogel composite material and tertiary repair of the carbon aerogel composite material in sequence, to obtain ablation-resistant and heat-insulating carbon aerogel composite material; in the secondary repair and tertiary repair, the preparation of the repair solution is: phenolic resin (phenolic resin THC-400), hexamethylenetetramine, ethylene glycol and deionized water are uniformly mixed in a mass ratio of 20:1.5:90:0.1 to obtain a repair solution.
[0100] Comparative Example 5
[0101] Comparative Example 5 is substantially the same as Example 1, except that:
[0102] ③ Prepare the repair solution, mix phenolic resin (phenolic resin THC-400), sodium carbonate, ethylene glycol and polyethylene glycol 400 in a mass ratio of 1:0.1:5:0.5 to obtain a repair solution; place the pretreated carbon aerogel composite material into the repair solution for vacuum impregnation for 30 minutes (the vacuum impregnation temperature is 25°C and the pressure is 5 kPa), then heat it at 80°C for 5 hours to form a gel, then age it at 180°C for 5 hours, and then heat it to 800°C under argon gas protection and carbonize it for 2 hours at a heating rate of 5°C / min to achieve a one-time nano-repair of the carbon aerogel composite material.
[0103] The present invention performs performance tests on the ablation-resistant and heat-insulating carbon aerogel composite materials prepared in various embodiments and comparative examples. The performance test results are shown in Table 1.
[0104] Table 1
[0105]
[0106]
[0107] Parts of the present invention that are not described in detail are well known to those skilled in the art.
[0108] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing an ablation-resistant and heat-insulating carbon aerogel composite material, characterized in that: The preparation method comprises the following steps: (1) A phenolic resin, a curing agent, a solvent and a dispersant are uniformly mixed to obtain a first phenolic solution, a fiber braid is impregnated with the first phenolic solution, and then the fiber braid is aged, dried and carbonized in sequence to obtain a carbon aerogel composite material; in step (1): the mass ratio of the phenolic resin, the curing agent, the solvent and the dispersant is 20:(1-5):(80-120):(0-1); (2) Phenolic resin, phenolic aerogel powder, dispersant and solvent are uniformly mixed to obtain a second phenolic solution, the carbon aerogel composite material is impregnated with the second phenolic solution and then allowed to stand, and then pre-carbonized at 400-600° C. to obtain a pre-treated carbon aerogel composite material; the phenolic aerogel powder is obtained by aging, drying, grinding and sieving the first phenolic solution in sequence; in step (2): the mass ratio of the phenolic resin, phenolic aerogel powder, dispersant and solvent is 1:(0.1-1):(0.1-0.5):(5-10); (3) The phenolic resin, curing agent, solvent and dispersant are mixed evenly to obtain a repair solution, and the pretreated carbon aerogel composite material is impregnated with the repair solution once, and then ultrasonically treated and impregnated twice, and finally gelled, aged and carbonized in sequence; in step (3): the mass ratio of the phenolic resin, curing agent, solvent and dispersant is 1:(0.1~0.5):(1~10):(0~1); (4) Repeat steps (2) and (3) 2 to 5 times in sequence to obtain an ablation-resistant and heat-insulating carbon aerogel composite material.
2. The preparation method according to claim 1, characterized in that: In step (1): The curing agent is one or more of paraformaldehyde, hexamethylenetetramine, aniline, formaldehyde, melamine, carbonate, bicarbonate and alkali.
3. The preparation method according to claim 1, characterized in that: In step (1): The solvent is one or more of anhydrous ethanol, propanol, methanol and ethylene glycol.
4. The preparation method according to claim 1, characterized in that: In step (1): The dispersant is one or more of deionized water, polyethylene glycol 400, polyethylene glycol 600 and polyethylene glycol 1000.
5. The preparation method according to claim 1, characterized in that: In step (1): The impregnation is atmospheric pressure impregnation or vacuum impregnation, and the pressure of the vacuum impregnation is 0.01~10kPa; The immersion time is 30 to 60 minutes.
6. The preparation method according to claim 1, characterized in that: In step (1): The aging is carried out at 120-150° C. for 5-30 hours.
7. The preparation method according to claim 1, characterized in that: In step (1): The drying is performed at 170-190° C. for 10-20 hours.
8. The preparation method according to claim 1, characterized in that: In step (1): The carbonization is carried out under vacuum conditions or under the protection of an inert gas; The carbonization temperature is 600-1200° C., and the carbonization time is 1.5-3.5 hours.
9. The preparation method according to claim 1, characterized in that: In step (1): The fiber braided body adopts one or more of carbon fiber, quartz fiber, glass fiber, mullite fiber and phenolic fiber.
10. The preparation method according to claim 1, characterized in that: In step (1): The fiber braided body has a structure of a needle-punched structure, a mesh structure, a 2.5D braided structure or a three-dimensional braided structure.
11. The preparation method according to claim 1, characterized in that: In step (2): The dispersant is one or more of triethylhexyl phosphoric acid, sodium lauryl sulfate, methyl amyl alcohol, and polyacrylamide.
12. The preparation method according to claim 1, characterized in that: In step (2): The solvent is one or more of anhydrous ethanol, propanol, methanol and ethylene glycol.
13. The preparation method according to claim 1, characterized in that: In step (2): The particle size of the phenolic aerogel powder is 100-200 meshes.
14. The preparation method according to claim 1, characterized in that: In step (2): The impregnation is normal pressure impregnation; The immersion time is 0.5 to 1 hour.
15. The preparation method according to claim 1, characterized in that: In step (2): The standing time is 0.5 to 2 hours.
16. The preparation method according to claim 1, characterized in that: In step (3): The curing agent is one or more of paraformaldehyde, hexamethylenetetramine, aniline, formaldehyde, melamine, carbonate, bicarbonate and alkali.
17. The preparation method according to claim 1, characterized in that: In step (3): The solvent is one or more of anhydrous ethanol, propanol, methanol and ethylene glycol.
18. The preparation method according to claim 1, characterized in that: In step (3): The dispersant is one or more of deionized water, polyethylene glycol 400, polyethylene glycol 600 and polyethylene glycol 1000.
19. The preparation method according to claim 1, characterized in that: In step (3): The first impregnation and the second impregnation are atmospheric pressure impregnation or vacuum impregnation, and the pressure of the vacuum impregnation is 0.01-10 kPa; The time of the first immersion is 30 to 60 minutes; The secondary impregnation time is 10 to 30 minutes.
20. The preparation method according to claim 1, characterized in that: In step (3): The ultrasonic treatment time is 15 to 30 minutes.
21. The preparation method according to claim 1, characterized in that: In step (3): The gel is gelled at 80-100° C. for 2-5 hours.
22. The preparation method according to claim 1, characterized in that: In step (3): The aging is carried out at 150-180° C. for 5-10 hours.
23. The preparation method according to claim 1, characterized in that: In step (3): The carbonization is carried out under vacuum conditions or under the protection of an inert gas; The carbonization temperature is 600-1200° C., and the carbonization time is 1.5-3.5 hours.
24. An ablation-resistant and heat-insulating carbon aerogel composite material prepared by the preparation method according to any one of claims 1 to 23.
Citation Information
Patent Citations
Repair coating for aerogel surface defects as well as preparation method and application of repair coating
CN114479602A
Modified high-temperature-ablation-resistant heat-insulation composite material and preparation method thereof
CN115850906A
Cited By
Polyacrylonitrile-itaconic acid fibrofelt reinforced carbon aerogel composite material as well as preparation method and application thereof
CN119569475A
A polyacrylonitrile-itaconic acid fiber felt reinforced carbon aerogel composite material, its preparation method and application
CN119569475B