Double-oil-resistant cable material and preparation method thereof
The dual oil-resistant cable material prepared by irradiation polymerization combines a variety of resins and flame retardants to solve the problem of insufficient dual oil-resistant, flame-resistant and high-temperature aging performance of existing oil-resistant cable materials, achieving high performance and low performance Toxicity and good processing performance.
Patent Information
- Application Number
- CN202411094716.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-10
- Publication Date
- 2024-12-03
AI Technical Summary
The existing oil-resistant cable materials have shortcomings in dual oil resistance, flame retardant properties and high-temperature aging properties. Chemical cross-linking methods lead to pimples of material, and the flame retardant antimony trioxide leads to large smoke production, which cannot meet the requirements of low toxicity.
The dual oil-resistant cable material is prepared by irradiation polymerization. By placing ethyl acrylate liquid in a cobalt source irradiation device for irradiation polymerization, combined with ethylene-vinyl acetate copolymer, maleic anhydride grafting agent, polyolefin resin and flame retardant Components such as agents are added, crosslinking agent, antioxidant and lubricant are added, and cable material is obtained after kneading, extrusion, cooling, pelletizing and drying.
It realizes dual oil resistance, low toxicity, low smoke, halogen-free flame retardant properties, meets Class A combustion requirements, improves the impact, low temperature resistance, stress cracking and heat cracking resistance of cable materials, has good processing performance, and avoids materials The appearance of pimples.
Smart Images

Figure BDA0004987553290000041 
Figure BDA0004987553290000061 
Figure BDA0004987553290000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cable materials, and in particular relates to a double oil-resistant cable material and a preparation method thereof. Background Art
[0002] With the rapid development of urban transportation systems such as subways and light rails, the demand for rolling stock cables has gradually increased. In order to reduce the risk of fire on rail lines, strengthening the safety of rolling stock cable operation has become an inevitable requirement for the development of rail transportation. Therefore, the development of low-smoke, halogen-free, flame-retardant cable materials with excellent oil resistance, high temperature resistance, mechanical and electrical properties has become the development direction of rolling stock cables.
[0003] First, some oil-resistant cable materials can only withstand mineral oil or fuel oil, and do not have dual oil resistance. Secondly, because the European standard locomotive cables do not have high requirements for flame retardancy, the general limit oxygen index is around 28-30. Furthermore, some dual oil-resistant materials do not have high requirements for aging performance at high temperatures, which also limits the application of locomotive cables.
[0004] In addition, some oil-resistant cable materials basically meet the requirements of oil resistance and flame retardancy, but there are still deficiencies in environmental protection and processing methods. For example, CN202111300377.5 discloses a chemically cross-linked double oil-resistant, low-temperature-resistant, low-smoke, halogen-free flame-retardant sheath material and its preparation method. The invented product has low hardness and can maintain flexibility at a low temperature of -40°C, has good flame retardant properties, and is excellent in resistance to minerals and fuel. Although the patent meets the standards of locomotive materials such as oil resistance, mechanical properties, and flame retardant properties, its formula adopts a chemical cross-linking method, which is prone to cross-linking during the extrusion process, resulting in lumps in the material, resulting in unqualified cable products; due to the addition of flame retardant antimony trioxide to the system, it cannot achieve the characteristics of low toxicity, and produces a lot of smoke. Summary of the invention
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a double oil-resistant cable material, comprising the following steps:
[0006] Step 1: Vacuum the ethyl acrylate liquid, and then place it in a cobalt source irradiation device for irradiation polymerization at a temperature of 25-35°C, with a radiation dose of 5-15 kGy and a dose rate of 5-8 kGy / h to obtain cured polyethyl acrylate. At this time, the polyethyl acrylate is a jelly-like elastic and soft cured product.
[0007] Step 2: Mix ethylene-vinyl acetate copolymer, maleic anhydride grafting agent, polyolefin resin and the above-mentioned polyethyl acrylate according to a ratio, and then add a flame retardant, a cross-linking agent, an antioxidant and a lubricant to obtain a mixed material;
[0008] Step 3: kneading, extruding, cooling, pelletizing and drying the mixed material to obtain a double oil-resistant cable material.
[0009] As a preferred embodiment of the above technical solution, the ethylene-vinyl acetate copolymer includes ethylene-vinyl acetate copolymer with model number 40LW and ethylene-vinyl acetate copolymer with model number UL00328 produced by Taiwan Polymer, the ratio of ethylene-vinyl acetate copolymer with model number 40LW and ethylene-vinyl acetate copolymer with model number UL00328 is 12:15, wherein the VA content in the ethylene-vinyl acetate copolymer with model number 40LW is 41%, and the VA content in the ethylene-vinyl acetate copolymer with model number UL00328 is 27.5%; the maleic anhydride grafting agent is MC312 or H268 of Ningbo Energy Light, and the grafting rate is greater than 0.8%; the polyolefin resin is Dow Chemical HDPE 3364NT; the flame retardant is formed by a compound of aluminum hydroxide and magnesium hydroxide, wherein the weight ratio of aluminum hydroxide to magnesium hydroxide is 4:1; the auxiliary cross-linking agent (radiation sensitizer) is TMPTMA or TAIC; the antioxidant includes hindered phenol antioxidant 1010 and thioester antioxidant DLTP, and the weight ratio of hindered phenol antioxidant 1010 to thioester antioxidant DLTP is 2:1; the lubricant is a silicone masterbatch, the silicone content of the silicone masterbatch is not less than 60%, and the carrier is ethylene propylene diene monomer rubber (EPDM).
[0010] As a preferred embodiment of the above technical solution, the mixed material in the step 2 contains 15-30 parts of ethylene-vinyl acetate copolymer, 2-10 parts of maleic anhydride grafting agent, 5-15 parts of polyolefin resin, 5-15 parts of polyethyl acrylate, 40-65 parts of flame retardant, 0.5-2 parts of co-crosslinking agent, 0.2-1 parts of antioxidant, and 0.5-2 parts of lubricant.
[0011] As a preferred embodiment of the above technical solution, the mixed material in the step 2 contains 27 parts of ethylene-vinyl acetate copolymer, 5 parts of maleic anhydride grafting agent, 10 parts of polyolefin resin, 5 parts of polyethyl acrylate, 50 parts of flame retardant, 1 part of co-crosslinking agent, 0.8 parts of antioxidant, and 1.2 parts of lubricant.
[0012] The double oil-resistant cable material is prepared using the above-mentioned preparation method.
[0013] The beneficial effects of the present invention are as follows: the present invention uses EVA (ethylene-vinyl acetate copolymer) resins with various VA (ethyl acetate) contents to adjust the performance of the cable material. Double oil resistance is achieved by the preparation and modification of EVA resin and polyolefin resin. With ethylene-vinyl acetate copolymer (EVA) and radiation-cured polyethyl acrylate and olefin resin as the matrix resin, the oil resistance, impact resistance, low temperature resistance, stress cracking resistance and aging resistance of the product are effectively improved. The addition of flame retardant can effectively improve the ablation resistance and flame retardant properties of the sheath material and prevent the spread of fire in a fire environment. Maleic anhydride grafting agent can serve as a "bridge" connecting organic matter and inorganic matter, effectively promote the blending of various components, and as a compatibilizer, give the final product good performance. The lubricant makes the surface of the product smooth and delicate, eliminates surface burrs, and improves processing performance. In combination with a cross-linking aid, an antioxidant, and a lubricant, an oil-resistant locomotive cable material is finally prepared. Double oil-resistant cable materials have excellent comprehensive performance, superior mechanical properties, high toughness, good resistance to high and low temperatures, high temperature aging, and heat cracking, double oil resistance, low toxicity index, meet the combustion requirements of Class A combustion grade, and have good extrusion processing performance. DETAILED DESCRIPTION
[0014] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0015] Embodiment 1:
[0016] The present invention provides a double oil-resistant cable material and a preparation method thereof. The components are as follows by weight:
[0017]
[0018] Among them, ethylene-vinyl acetate copolymer is a compound of Mitsui Dow's 40LX and ExxonMobil's UL00328, with a ratio of 12:15, of which the VA content of 40LX is 41%, and the VA content of UL00328 is 27%; the polyolefin resin is Dow Chemical HDPE3364NT; the maleic anhydride grafting agent is Ningbo Energy Light's MC312 or H268, and the grafting rate is greater than 0.8%; the radiation dose used for radiation curing of polyethyl acrylate is 5-15KGy; the flame retardant used is a magnesium-aluminum compound, the aluminum hydroxide is Luoyang Rhine Aluminum (LY-01PM), and the magnesium hydroxide model is Niko A7, wherein the ratio of aluminum to magnesium is 4:1; the auxiliary cross-linking agent (radiation sensitizer) is TMPTMA or TAIC, which can promote the cross-linking of the cable during electron beam irradiation; the antioxidant is a mixture of hindered phenol 1010 and thioester DLTP, and the weight ratio of the main and auxiliary antioxidants is 2:1; the lubricant is a silicone masterbatch, the silicone content of the silicone masterbatch is not less than 60%, and the carrier is EPDM.
[0019] The specific steps are as follows:
[0020] By weight, take 27 parts of ethylene-vinyl acetate copolymer, 5 parts of polyethyl acrylate, 10 parts of polyolefin resin, and 5 parts of maleic anhydride grafting agent, accurately measure and put them into a high-speed mixer, run at low speed for 3 minutes, then accurately weigh 50 parts of flame retardant, 1 part of radiation sensitizer, 0.8 parts of hindered phenol antioxidant 1010 and 0.8 parts of thioester antioxidant DLTP, and 1.2 parts of lubricant in a mixing kettle, and mix at high speed for 1 minute.
[0021] The mixed raw materials are plasticized uniformly in an internal mixer, sent to a double-cone feeding hopper through an elevator, processed by a two-stage extruder, plasticized by a twin-screw extruder at 1250rpm, and then transferred to a pelletizer by a single-screw extruder at 750rpm for cooling and packaging.
[0022] Embodiment 2:
[0023] The difference from Example 1 is that the number of polyethyl acrylate is increased to 8 parts, and the number of ethylene-vinyl acetate copolymer 40LW and UL00328 is reduced. By weight, the ratio is 9:15, totaling 24 parts. The rest is the same as Example 1.
[0024] Embodiment 3:
[0025] The difference from Example 1 is that the number of polyethyl acrylate is increased to 15 parts, and the number of ethylene-vinyl acetate copolymer 40LW and UL00328 is reduced. By weight, the ratio is 7:15, totaling 22 parts. The rest is the same as Example 1.
[0026] Embodiment 4:
[0027] The difference from Example 1 is that the amount of polyethylene used is reduced by 3 parts, and the reduced amount is added to the amount of polyethyl acrylate, and the rest is the same as Example 1.
[0028] Embodiment 5:
[0029] The difference from Example 1 is that the amount of polyethylene used is reduced by 3 parts, and the reduced amount is added to the amount of polyethyl acrylate, and the rest is the same as Example 1.
[0030] Embodiment 6:
[0031] The difference from Example 1 is that all the flame retardants used are aluminum hydroxide.
[0032] Embodiment 7:
[0033] The difference between Example 7 and Example 1 is that the ratio of the flame retardants aluminum hydroxide and magnesium hydroxide used is 3:2.
[0034] The physicochemical properties of the cable prepared in Example 1 were tested, and the test results are as follows:
[0035]
[0036]
[0037] It is worth mentioning that the technical features such as the high-mix kettle involved in the patent application of the present invention should be regarded as the prior art. The specific structure, working principle and possible control method and spatial layout method of these technical features can be selected by conventional methods in the field, and should not be regarded as the inventive point of the present patent. The present patent will not be further elaborated.
[0038] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in this field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in this technical field through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the existing technology should be within the scope of protection determined by the claims.
Claims
1. A method for preparing a double oil-resistant cable material, characterized in that: The following steps are included: Step 1, vacuuming the ethyl acrylate liquid, and then placing it in a cobalt source irradiation device for irradiation polymerization at a temperature of 25-35° C., irradiating with a radiation dose of 5-15 kGy, and a dose rate of 5-8 kGy / h to obtain cured polyethyl acrylate; Step 2: Mix ethylene-vinyl acetate copolymer, maleic anhydride grafting agent, polyolefin resin and the above-mentioned polyethyl acrylate according to a ratio, and then add a flame retardant, a cross-linking agent, an antioxidant and a lubricant to obtain a mixed material; Step 3: kneading, extruding, cooling, pelletizing and drying the mixed material to obtain a double oil-resistant cable material.
2. The method for preparing a double oil resistant cable material according to claim 1, characterized in that: The ethylene-vinyl acetate copolymer includes ethylene-vinyl acetate copolymer with model number 40LW and ethylene-vinyl acetate copolymer with model number UL00328 produced by Formosa Polymer Technology, the ratio of ethylene-vinyl acetate copolymer with model number 40LW and ethylene-vinyl acetate copolymer with model number UL00328 is 12:15, wherein the VA content in ethylene-vinyl acetate copolymer with model number 40LW is 41%, and the VA content in ethylene-vinyl acetate copolymer with model number UL00328 is 27.5%; the maleic anhydride grafting agent is MC312 or H268 produced by Ningbo Energy Light, and the grafting rate is greater than 0.8%; the polyolefin resin is Dow Chemical HDPE 3364NT; the flame retardant is formed by a compound of aluminum hydroxide and magnesium hydroxide, wherein the weight ratio of aluminum hydroxide to magnesium hydroxide is 4:1; the auxiliary cross-linking agent is TMPTMA or TAIC; the antioxidant includes hindered phenol antioxidant 1010 and thioester antioxidant DLTP, and the weight ratio of hindered phenol antioxidant 1010 to thioester antioxidant DLTP is 2:1; the lubricant is a silicone masterbatch, the silicone content of the silicone masterbatch is not less than 60%, and the carrier is ethylene propylene diene rubber.
3. The method for preparing a double oil resistant cable material according to claim 2, characterized in that: The mixture in step 2 comprises 15-30 parts of ethylene-vinyl acetate copolymer, 2-10 parts of maleic anhydride grafting agent, 5-15 parts of polyolefin resin, 5-15 parts of polyethyl acrylate, 40-65 parts of flame retardant, 0.5-2 parts of auxiliary crosslinking agent, 0.2-1 parts of antioxidant and 0.5-2 parts of lubricant.
4. The method for preparing a double oil resistant cable material according to claim 3, characterized in that: The mixture in step 2 contains 27 parts of ethylene-vinyl acetate copolymer, 5 parts of maleic anhydride grafting agent, 10 parts of polyolefin resin, 5 parts of polyethyl acrylate, 50 parts of flame retardant, 1 part of co-crosslinking agent, 0.8 parts of antioxidant and 1.2 parts of lubricant.
5. Double oil-resistant cable material, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 4.
Citation Information
Patent Citations
Double-oil-resistant high-flame-retardant high-temperature-resistant irradiation crosslinking composition as well as preparation method and application thereof
CN114133649A