A parameter optimization method for the production and processing of wear-resistant ceramic glazes

By adding metal tungsten and carbon fibers to silicon nitride ceramic materials, using the pneumatic sintering process to optimize parameters and regulate microstructure, the problem of brittle fracture of silicon nitride ceramic materials is solved, and its fracture toughness and friction wear performance are improved, satisfying the metallurgy field application requirements.

CN118675671BActive Publication Date: 2024-11-15JIANGXI QIANTAO NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411144989.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-15
Estimated Expiration
2044-08-20

AI Technical Summary

Technical Problem

Silicon nitride ceramic materials are prone to brittle fracture during use, resulting in the suspension of production lines. How to improve their fracture toughness while maintaining their high wear and corrosion resistance has become a key issue.

Method used

By adding metal tungsten and carbon fibers as reinforced phases to silicon nitride ceramic materials, the parameters are optimized using the pneumatic sintering process, and step by step heating, pressurization and cooling are carried out to prepare multiphase composite materials, regulate microstructure, and improve the mechanics of the materials. performance.

Benefits of technology

The fracture toughness and friction wear performance of silicon nitride ceramic materials have been significantly improved, meeting the practical application needs of the metallurgy field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118675671B_ABST
    Figure CN118675671B_ABST
Patent Text Reader

Abstract

The present invention discloses a parameter optimization method for the production and processing of wear-resistant ceramic glaze, which relates to the technical field of ceramic processing, including: weighing the original powder according to a set ratio and pre-treating the raw materials; obtaining the influencing parameters of each stage in the gas pressure sintering process; using the gas pressure sintering process to conduct a control experiment; outputting the control experiment with the highest shape retention rate corresponding to the influencing parameters of each stage as the optimal parameter group; calculating the low-destructive sample performance and high-destructive sample performance of each group of second ceramic samples; using a weight distribution formula to calculate the performance score of each group of second ceramic samples, outputting the second control experiment with the highest performance score corresponding to the original powder ratio as the optimal ratio; judging whether the performance score of the second ceramic sample under the optimal ratio is higher than the set score threshold. Through the control of various parameters of production and processing, the optimal values ​​of the influencing parameters of each stage in the gas pressure sintering process are calculated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic processing, and in particular to a parameter optimization method for production and processing of wear-resistant ceramic glaze. Background Art

[0002] As an inorganic non-metallic material, silicon nitride ceramic material has excellent performance characteristics such as high hardness, high temperature resistance, high wear resistance, corrosion resistance, insulation and a small thermal expansion coefficient. At the same time, the adhesion between silicon nitride ceramic material and steel is small, and it shows excellent self-lubricating effect under long-term sliding friction; because silicon nitride ceramic material has a small thermal expansion coefficient, it can still maintain stable material properties in harsh working environments with sudden heating and cooling. Therefore, silicon nitride ceramic material is particularly suitable for use under high speed, high temperature, severe wear and other working conditions, and is very suitable for the production and application of wear-resistant parts in the metallurgical industry.

[0003] However, a major disadvantage of silicon nitride ceramics, which have excellent properties such as high wear resistance and corrosion resistance, is that they have high brittleness. Compared with traditional metal materials, silicon nitride ceramic products are prone to brittle fracture during use, resulting in the suspension of related production lines. Even so, silicon nitride ceramic guide rollers still show a longer service life than traditional metals in the corresponding production lines. Therefore, how to improve the fracture toughness of silicon nitride ceramic materials while effectively ensuring the advantages of silicon nitride ceramic materials such as high wear resistance and corrosion resistance has become a key issue that needs to be solved at this stage. Summary of the invention

[0004] In order to solve the above technical problems, a parameter optimization method for the production and processing of wear-resistant ceramic glazes is provided. This technical solution solves the problems raised in the above background technology.

[0005] In order to achieve the above purpose, the technical solution adopted by the present invention is:

[0006] A parameter optimization method for production and processing of wear-resistant ceramic glazes, comprising:

[0007] The raw powder is weighed according to a set ratio and pre-processed, wherein the raw powder includes silicon nitride ceramics, basic sintering aid alumina, reinforcing phase metal tungsten and carbon fiber;

[0008] Obtaining the influencing parameters of each stage in the gas pressure sintering process, wherein the influencing parameters include heating rate, stage pressure, holding temperature, holding time and cooling rate;

[0009] Based on the changes of the influencing parameters at each stage, the powder is heated, pressurized and cooled step by step using a gas pressure sintering process, and at least one group of first control experiments is performed to obtain each group of first ceramic samples;

[0010] Calculate the shape retention rate of the first ceramic sample in each group, and output the influencing parameters of each stage corresponding to the first control experiment with the highest shape retention rate as the optimal parameter group;

[0011] Based on the change of the original powder ratio, at least one group of second control experiments of the gas pressure sintering process is carried out using the optimal parameter group to obtain each group of second ceramic samples;

[0012] By performing a low-destructive test on each group of second ceramic samples, the low-destructive sample performance of each group of second ceramic samples is calculated, wherein the low-destructive sample performance is sample relative density, Vickers hardness and wear resistance;

[0013] By performing a high-destructive test on each group of second ceramic samples, the high-destructive sample performance of each group of second ceramic samples is calculated, wherein the high-destructive sample performance is bending strength and fracture toughness;

[0014] Based on the low-destructive sample performance and high-destructive sample performance of each group of second ceramic samples, the performance score of each group of second ceramic samples is calculated using a weight distribution formula, and the second control experiment with the highest output performance score corresponds to the original powder ratio as the optimal ratio;

[0015] It is determined whether the performance score of the second ceramic sample under the optimal ratio is higher than the set score threshold. If so, no output is made; if not, the original powder ratio is reset and a third control experiment of the gas pressure sintering process is performed.

[0016] Preferably, the weighing of the raw powder according to a set ratio and the pretreatment of the raw materials specifically include:

[0017] Set the original powder ratio and ball milling time;

[0018] Pour the original powder, grinding balls and ball-milling medium anhydrous ethanol into the ball mill according to the set original powder ratio;

[0019] Fix the ball mill on the turntable and perform ball milling in forward and reverse directions alternately within the set ball milling time;

[0020] The ball-milled slurry is placed in an industrial drying oven and dried at 60°C until the anhydrous ethanol is basically evaporated;

[0021] The dried blank is placed in a pulverizer for pulverization, and then passed through a 50-mesh and a 100-mesh sieve in turn for sieving and granulation.

[0022] Preferably, the powder is heated, pressurized and cooled step by step by using a gas pressure sintering process based on the changes in the influencing parameters at each stage, and at least one group of first control experiments is performed to obtain each group of first ceramic samples, which specifically includes:

[0023] Set the influencing parameter values ​​of each stage of each group of control experiments;

[0024] Introduce nitrogen into the sintering furnace to raise the pressure inside the furnace to the first stage pressure;

[0025] The temperature is raised to a first insulation temperature at a first heating rate, and the insulation time is set to the first insulation time;

[0026] Continue to introduce nitrogen to pressurize to the second stage pressure;

[0027] The temperature is raised to a second insulation temperature at a second heating rate, and the insulation time is set to the second insulation time;

[0028] The temperature is raised to a third insulation temperature at a third heating rate, and the insulation time is set to the third insulation time;

[0029] Cooling the temperature to a fourth insulation temperature at a first cooling rate, and setting the insulation time to a fourth insulation time;

[0030] Cooling the temperature to the fifth insulation temperature at the second cooling rate, and the insulation time is set to the fifth insulation time;

[0031] The sintering furnace is cooled down naturally to room temperature, and the pressure inside the furnace is reduced to normal pressure;

[0032] The furnace is opened and the first ceramic samples of each group that have been sintered are taken out.

[0033] Preferably, the step of calculating the shape retention rate of each group of first ceramic samples and outputting the influencing parameters of each stage corresponding to the first control experiment with the highest shape retention rate as the optimal parameter group specifically includes:

[0034] Modeling each group of first ceramic samples to obtain each group of first ceramic sample models;

[0035] Obtain standard ceramic models;

[0036] The shape retention rate of each group of first ceramic samples is calculated using the shape retention rate formula;

[0037] The influencing parameters of each stage corresponding to the first control experiment with the highest output shape retention rate are the optimal parameter groups;

[0038] The shape retention rate formula includes:

[0039]

[0040] In the formula, is the shape retention rate of the first ceramic sample in group i, is the overlapping volume of the first ceramic sample model and the standard ceramic model of the i-th group, is the total volume of the standard ceramic model.

[0041] Preferably, the calculating the low-destructive sample performance of each group of second ceramic samples by performing a low-destructive test on each group of second ceramic samples specifically includes:

[0042] The volume density of the second ceramic sample in each group was calculated using the water displacement method;

[0043] Calculating the sample relative density of each group of second ceramic samples using a relative density formula based on the volume density of each group of second ceramic samples;

[0044] The second ceramic samples of each group are placed directly under the diamond indenter of the Vickers hardness tester, and the normal load and stress time are set;

[0045] Take at least two different areas for hardness testing;

[0046] Observe the surface indentation through an optical microscope and record the diagonal length of the corresponding indentation;

[0047] Calculating the Vickers hardness of each group of second ceramic samples using a Vickers hardness calculation formula;

[0048] Commercial silicon nitride ceramic balls are used as friction devices;

[0049] Set the friction normal load, sliding frequency, friction stroke and friction time;

[0050] Conducting friction test on at least one location of each group of second ceramic samples by dry sliding reciprocating friction method;

[0051] measuring the friction coefficient of the surface of each group of second ceramic samples after the friction test;

[0052] The wear resistance of each group of second ceramic samples is calculated using the wear resistance formula;

[0053] The sample relative density, Vickers hardness and wear resistance of each group of second ceramic samples are combined and output as low-destructive sample performance of each group of second ceramic samples;

[0054] The bulk density is:

[0055]

[0056] In the formula, is the volume density of the second ceramic sample in the i-th group, is the mass of the second ceramic sample in the i-th group, is the mass of the second ceramic sample in group i after absorbing water, is the floating weight of the second ceramic sample in group i, is the density of distilled water;

[0057] The relative density formula is:

[0058]

[0059] In the formula, is the relative density of the second ceramic sample in group i, is the volume density of the second ceramic sample in the i-th group, is the theoretical density of the ceramic sample;

[0060] The Vickers hardness calculation formula is:

[0061]

[0062] In the formula, is the Vickers hardness of the second ceramic sample in group i, To set the normal load, is the arithmetic mean of the diagonal lengths of the surface indentations of the second ceramic sample in the i-th group;

[0063] The wear resistance formula is:

[0064]

[0065] In the formula, is the wear resistance of the second ceramic sample in group i, is the friction coefficient of the second ceramic sample at the jth position in the i-th group, The number of friction tests performed on the second ceramic sample of the i-th group.

[0066] Preferably, the calculating the high-destructive sample performance of each group of second ceramic samples by performing a high-destructive test on each group of second ceramic samples specifically includes:

[0067] Cut off a portion of each group of second ceramic samples and process them into two rectangular parallelepiped samples of set sizes;

[0068] The three-point bending method is used to apply pressure to the two ends and the middle of one of the rectangular samples in each group;

[0069] The maximum load just before the sample breaks is recorded as the first breaking load;

[0070] Calculating the bending strength of each group of second ceramic samples using a bending strength formula;

[0071] The single-edge notched beam method was used to make a small notch in the middle of one of the rectangular samples in each group as a pre-set crack;

[0072] Apply pressure to both ends of the rectangular sample and record the maximum load just before the sample breaks as the second breaking load;

[0073] The fracture toughness of each group of second ceramic samples is calculated using the fracture toughness formula;

[0074] The bending strength and fracture toughness of each group of second ceramic samples are combined and output as high destructive sample properties of each group of second ceramic samples;

[0075] The bending strength formula is:

[0076]

[0077] In the formula, is the flexural strength of the second ceramic sample in group i, is the first fracture load of the second ceramic sample in the i-th group, is the length of the cuboid sample, is the height of the cuboid sample, is the width of the rectangular sample;

[0078] The fracture toughness formula is:

[0079]

[0080] In the formula, is the fracture toughness of the second ceramic sample in group i, is the second fracture load of the second ceramic sample in group i, is the incision length.

[0081] Preferably, the performance scores of the second ceramic samples of each group are calculated by using a weight distribution formula based on the low-destructive sample performance and the high-destructive sample performance of each group, and the second control experiment with the highest performance score is output as the optimal ratio of the original powder material, specifically comprising:

[0082] Obtaining the score weights of each low-destructive sample performance and high-destructive sample performance;

[0083] Calculate the performance score of each group of second ceramic samples using a weight distribution formula based on the score weight;

[0084] The second control experiment with the highest output performance score corresponds to the optimal ratio of original powder material;

[0085] The weight distribution formula is:

[0086]

[0087] In the formula, is the performance score of the second ceramic sample in group i, , , , , They are the relative density, Vickers hardness, wear resistance, bending strength and fracture toughness of the samples, , , , , They are the score weights of sample relative density, Vickers hardness, wear resistance, bending strength and fracture toughness respectively.

[0088] Preferably, the step of judging whether the performance score of the second ceramic sample at the optimal ratio is higher than a set score threshold specifically includes:

[0089] Obtaining a performance score of the second ceramic sample at the optimal ratio;

[0090] Set scoring thresholds;

[0091] It is determined whether the performance score of the second ceramic sample under the optimal ratio is higher than the set score threshold. If so, no output is made. If not, the original powder ratio is reset and the third control experiment of the gas pressure sintering process is carried out.

[0092] Compared with the prior art, the present invention has the following beneficial effects:

[0093] In response to the actual application needs of silicon nitride ceramics as wear-resistant materials in the metallurgical field, by adding one or more reinforcing phases to the ceramic material for toughening, metal tungsten and carbon fiber are combined as reinforcing phases and added to the silicon nitride ceramic material at a certain gradient to prepare a multiphase composite silicon nitride ceramic material, regulate the microstructure, and improve the mechanical properties of the silicon nitride ceramic material, especially the fracture toughness and friction and wear performance, to meet the needs of the actual production process. BRIEF DESCRIPTION OF THE DRAWINGS

[0094] Figure 1 It is a flow chart of the parameter optimization method for the production and processing of wear-resistant ceramic glaze of the present invention;

[0095] Figure 2 This is a flow chart of the raw material pretreatment method of the present invention;

[0096] Figure 3 The present invention is a flow chart of the gas pressure sintering process;

[0097] Figure 4 A flow chart of a method for calculating the shape retention rate of each group of first ceramic samples of the present invention;

[0098] Figure 5 A flow chart of a method for calculating low-destructive sample performance of each group of second ceramic samples of the present invention;

[0099] Figure 6 A flow chart of a method for calculating high destructive sample performance of each group of second ceramic samples of the present invention;

[0100] Figure 7The second control experiment with the highest output performance score of the present invention corresponds to an optimal ratio of the original powder ratio as a flow chart of the method;

[0101] Figure 8 The present invention is a flow chart of a method for determining whether the performance score of the second ceramic sample at the optimal ratio is higher than a set score threshold. DETAILED DESCRIPTION

[0102] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.

[0103] Reference Figure 1 As shown, a parameter optimization method for the production and processing of wear-resistant ceramic glazes comprises:

[0104] The raw powder is weighed according to a set ratio and pre-processed, wherein the raw powder includes silicon nitride ceramics, basic sintering aid alumina, reinforcing phase metal tungsten and carbon fiber;

[0105] Obtaining the influencing parameters of each stage in the gas pressure sintering process, wherein the influencing parameters include heating rate, stage pressure, holding temperature, holding time and cooling rate;

[0106] Based on the changes of the influencing parameters at each stage, the powder is heated, pressurized and cooled step by step using a gas pressure sintering process, and at least one group of first control experiments is performed to obtain each group of first ceramic samples;

[0107] Calculate the shape retention rate of the first ceramic sample in each group, and output the influencing parameters of each stage corresponding to the first control experiment with the highest shape retention rate as the optimal parameter group;

[0108] Based on the change of the original powder ratio, at least one group of second control experiments of the gas pressure sintering process is carried out using the optimal parameter group to obtain each group of second ceramic samples;

[0109] By performing a low-destructive test on each group of second ceramic samples, the low-destructive sample performance of each group of second ceramic samples is calculated, wherein the low-destructive sample performance is sample relative density, Vickers hardness and wear resistance;

[0110] By performing a high-destructive test on each group of second ceramic samples, the high-destructive sample performance of each group of second ceramic samples is calculated, wherein the high-destructive sample performance is bending strength and fracture toughness;

[0111] Based on the low-destructive sample performance and high-destructive sample performance of each group of second ceramic samples, the performance score of each group of second ceramic samples is calculated using a weight distribution formula, and the second control experiment with the highest output performance score corresponds to the original powder ratio as the optimal ratio;

[0112] It is determined whether the performance score of the second ceramic sample under the optimal ratio is higher than the set score threshold. If so, no output is made; if not, the original powder ratio is reset and a third control experiment of the gas pressure sintering process is performed.

[0113] The third control experiment of the gas pressure sintering process has the same process as the second control experiment of the gas pressure sintering process.

[0114] Reference Figure 2 As shown, the raw powder is weighed according to the set ratio, and the raw material pretreatment is carried out, including:

[0115] Set the original powder ratio and ball milling time;

[0116] Pour the original powder, grinding balls and ball-milling medium anhydrous ethanol into the ball mill according to the set original powder ratio;

[0117] Fix the ball mill on the turntable and perform ball milling in forward and reverse directions alternately within the set ball milling time;

[0118] The ball-milled slurry is placed in an industrial drying oven and dried at 60°C until the anhydrous ethanol is basically evaporated;

[0119] The dried blank is placed in a pulverizer for pulverization, and then passed through a 50-mesh and a 100-mesh sieve in turn for sieving and granulation.

[0120] During the ball milling process, anhydrous ethanol can be used as a co-solvent to help reduce the viscosity of the material and improve the ball milling efficiency. At the same time, anhydrous ethanol can also prevent the material from agglomerating during the grinding process, ensuring that the ground material has good dispersibility.

[0121] Reference Figure 3 As shown, based on the changes in the influencing parameters at each stage, the powder is heated, pressurized and cooled step by step using the gas pressure sintering process, and at least one group of first control experiments is performed to obtain each group of first ceramic samples, which specifically include:

[0122] Set the influencing parameter values ​​of each stage of each group of control experiments;

[0123] Introduce nitrogen into the sintering furnace to raise the pressure inside the furnace to the first stage pressure;

[0124] The temperature is raised to a first insulation temperature at a first heating rate, and the insulation time is set to the first insulation time;

[0125] Continue to introduce nitrogen to pressurize to the second stage pressure;

[0126] The temperature is raised to a second insulation temperature at a second heating rate, and the insulation time is set to the second insulation time;

[0127] The temperature is raised to a third insulation temperature at a third heating rate, and the insulation time is set to the third insulation time;

[0128] Cooling the temperature to a fourth insulation temperature at a first cooling rate, and setting the insulation time to a fourth insulation time;

[0129] Cooling the temperature to the fifth insulation temperature at the second cooling rate, and the insulation time is set to the fifth insulation time;

[0130] The sintering furnace is cooled down naturally to room temperature, and the pressure inside the furnace is reduced to normal pressure;

[0131] The furnace is opened and the first ceramic samples of each group that have been sintered are taken out.

[0132] Gas pressure sintering is a specialized sintering process used primarily to produce advanced ceramic materials such as ultra-high temperature ceramics. The process involves a series of controlled heat treatments under an inert atmosphere (usually argon or nitrogen) and applying varying pressures to achieve material densification and eliminate porosity.

[0133] Reference Figure 4 As shown, the shape retention rate of each group of first ceramic samples is calculated, and the influencing parameters of each stage corresponding to the first control experiment with the highest shape retention rate are output as the optimal parameter group, specifically including:

[0134] Modeling each group of first ceramic samples to obtain each group of first ceramic sample models;

[0135] Obtain standard ceramic models;

[0136] The shape retention rate of each group of first ceramic samples is calculated using the shape retention rate formula;

[0137] The influencing parameters of each stage corresponding to the first control experiment with the highest output shape retention rate are the optimal parameter groups;

[0138] The shape retention rate formula includes:

[0139]

[0140] In the formula, is the shape retention rate of the first ceramic sample in group i, is the overlapping volume of the first ceramic sample model and the standard ceramic model of the i-th group, is the total volume of the standard ceramic model.

[0141] When conducting sintering tests on metal-ceramic composites with different ratios, the sintering temperature should increase with the increase of the mass proportion of ceramic powder in the ratio. The reason is that firstly, the sintering temperature of ceramic materials is higher than that of alloys. As the ratio of the two increases, the sintering temperature of the composite material will also increase. Secondly, during the sintering process, a large amount of liquid phase will be produced at the grain boundaries of the metal particles. As the metal content increases, the generation of this liquid phase will also increase. Finally, the shape retention rate of the composite material after sintering will decrease.

[0142] Reference Figure 5 As shown, by performing low-destructive tests on each group of second ceramic samples, calculating the low-destructive sample performance of each group of second ceramic samples specifically includes:

[0143] The volume density of the second ceramic sample in each group was calculated using the water displacement method;

[0144] Calculating the sample relative density of each group of second ceramic samples using a relative density formula based on the volume density of each group of second ceramic samples;

[0145] The second ceramic samples of each group are placed directly under the diamond indenter of the Vickers hardness tester, and the normal load and stress time are set;

[0146] Take at least two different areas for hardness testing;

[0147] Observe the surface indentation through an optical microscope and record the diagonal length of the corresponding indentation;

[0148] Calculating the Vickers hardness of each group of second ceramic samples using a Vickers hardness calculation formula;

[0149] Commercial silicon nitride ceramic balls are used as friction devices;

[0150] Set the friction normal load, sliding frequency, friction stroke and friction time;

[0151] Conducting friction test on at least one location of each group of second ceramic samples by dry sliding reciprocating friction method;

[0152] measuring the friction coefficient of the surface of each group of second ceramic samples after the friction test;

[0153] The wear resistance of each group of second ceramic samples is calculated using the wear resistance formula;

[0154] The sample relative density, Vickers hardness and wear resistance of each group of second ceramic samples are combined and output as low-destructive sample performance of each group of second ceramic samples;

[0155] The bulk density is:

[0156]

[0157] In the formula, is the volume density of the second ceramic sample in the i-th group, is the mass of the second ceramic sample in the i-th group, is the mass of the second ceramic sample in group i after absorbing water, is the floating weight of the second ceramic sample in group i, is the density of distilled water;

[0158] The relative density formula is:

[0159]

[0160] In the formula, is the relative density of the second ceramic sample in group i, is the volume density of the second ceramic sample in the i-th group, is the theoretical density of the ceramic sample;

[0161] The Vickers hardness calculation formula is:

[0162]

[0163] In the formula, is the Vickers hardness of the second ceramic sample in group i, To set the normal load, is the arithmetic mean of the diagonal lengths of the surface indentations of the second ceramic sample in the i-th group;

[0164] The wear resistance formula is:

[0165]

[0166] In the formula, is the wear resistance of the second ceramic sample in group i, is the friction coefficient of the second ceramic sample at the jth position in the i-th group, The number of friction tests performed on the second ceramic sample of the i-th group.

[0167] Hardness is an indicator to measure the hardness or softness of a material and is one of the most commonly used and critical mechanical properties of a material. Commonly used hardness test methods include Vickers hardness, Rockwell hardness, etc. Among them, Vickers hardness has the widest application range due to its wide test hardness range and high precision.

[0168] Reference Figure 6 As shown, by performing a high-destructive test on each group of second ceramic samples, the high-destructive sample performance of each group of second ceramic samples is calculated, which specifically includes:

[0169] Cut off a portion of each group of second ceramic samples and process them into two rectangular parallelepiped samples of set sizes;

[0170] The three-point bending method is used to apply pressure to the two ends and the middle of one of the rectangular samples in each group;

[0171] The maximum load just before the sample breaks is recorded as the first breaking load;

[0172] Calculating the bending strength of each group of second ceramic samples using a bending strength formula;

[0173] The single-edge notched beam method was used to make a small notch in the middle of one of the rectangular samples in each group as a pre-set crack;

[0174] Apply pressure to both ends of the rectangular sample and record the maximum load just before the sample breaks as the second breaking load;

[0175] The fracture toughness of each group of second ceramic samples is calculated using the fracture toughness formula;

[0176] The bending strength and fracture toughness of each group of second ceramic samples are combined and output as high destructive sample properties of each group of second ceramic samples;

[0177] The bending strength formula is:

[0178]

[0179] In the formula, is the flexural strength of the second ceramic sample in group i, is the first fracture load of the second ceramic sample in the i-th group, is the length of the cuboid sample, is the height of the cuboid sample, is the width of the rectangular sample;

[0180] The fracture toughness formula is:

[0181]

[0182] In the formula, is the fracture toughness of the second ceramic sample in group i, is the second fracture load of the second ceramic sample in group i, is the incision length.

[0183] It is very difficult to prefabricate an ideal primary crack on a refractory sample. Therefore, when using the single-sided notch beam method to test the fracture properties of the material, an artificial notch with a certain radius is usually prefabricated on the sample as a substitute. The artificial notch has a curvature radius much larger than that of the natural crack, which will cause the stress concentration to decrease. The measured fracture toughness value will be too large and will increase with the increase of the notch width. This effect is called the "notch passivation effect".

[0184] Reference Figure 7 As shown, based on the low-destructive sample performance and high-destructive sample performance of each group of second ceramic samples, the performance score of each group of second ceramic samples is calculated using a weight distribution formula, and the second control experiment with the highest output performance score corresponds to the optimal original powder ratio, specifically including:

[0185] Obtaining the score weights of each low-destructive sample performance and high-destructive sample performance;

[0186] Calculate the performance score of each group of second ceramic samples using a weight distribution formula based on the score weight;

[0187] The second control experiment with the highest output performance score corresponds to the optimal ratio of original powder material;

[0188] The weight distribution formula is:

[0189]

[0190] In the formula, is the performance score of the second ceramic sample in group i, , , , , They are the relative density, Vickers hardness, wear resistance, bending strength and fracture toughness of the samples, , , , , They are the score weights of sample relative density, Vickers hardness, wear resistance, bending strength and fracture toughness respectively.

[0191] Score weight refers to the importance of sample performance relative to the performance score. It is different from general proportion. It reflects not only the percentage of a certain factor or indicator, but emphasizes the relative importance of factors or indicators, tending to contribution or importance. Usually, weight can be judged and calculated by dividing indicators into multiple levels. Commonly used methods include hierarchical analysis method, fuzzy method, fuzzy hierarchical analysis method and expert evaluation method.

[0192] Reference Figure 8 As shown, judging whether the performance score of the second ceramic sample under the optimal ratio is higher than the set score threshold specifically includes:

[0193] Obtaining a performance score of the second ceramic sample at the optimal ratio;

[0194] Set scoring thresholds;

[0195] It is determined whether the performance score of the second ceramic sample under the optimal ratio is higher than the set score threshold. If so, no output is made. If not, the original powder ratio is reset and the third control experiment of the gas pressure sintering process is carried out.

[0196] Since it is not possible to include all possible values ​​of all parameters when setting up the control experiment, it is necessary to determine whether it is necessary to reset the original powder ratio and conduct a third control experiment of the gas pressure sintering process based on the performance score of the final sample.

[0197] Furthermore, the present solution also proposes a computer-readable storage medium on which a computer-readable program is stored. When the computer-readable program is called, the above-mentioned parameter optimization method for the production and processing of wear-resistant ceramic glaze is executed.

[0198] It is understandable that the storage medium may be a magnetic medium, such as a floppy disk, a hard disk, or a magnetic tape; an optical medium, such as a DVD; or a semiconductor medium, such as a solid state drive (SSD).

[0199] To sum up, the advantages of the present invention are: in response to the actual application needs of silicon nitride ceramics as wear-resistant materials in the metallurgical field, by adding one or more reinforcing phases to the ceramic material for combined toughening, metal tungsten and carbon fiber are combined as reinforcing phases and added to the silicon nitride ceramic material at a certain gradient to prepare a multiphase composite silicon nitride ceramic material, thereby regulating the microstructure and improving the mechanical properties of the silicon nitride ceramic material, especially the fracture toughness and friction and wear performance, to meet the needs of the actual production process.

[0200] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.

Claims

1. A parameter optimization method for the production and processing of wear-resistant ceramic glazes, characterized in that: include: The raw powder is weighed according to a set ratio and pre-processed, wherein the raw powder includes silicon nitride ceramics, basic sintering aid alumina, reinforcing phase metal tungsten and carbon fiber; Obtaining the influencing parameters of each stage in the gas pressure sintering process, wherein the influencing parameters include heating rate, stage pressure, holding temperature, holding time and cooling rate; Based on the changes of the influencing parameters at each stage, the powder is heated, pressurized and cooled step by step using a gas pressure sintering process, and at least one group of first control experiments is performed to obtain each group of first ceramic samples; Calculate the shape retention rate of the first ceramic sample in each group, and output the influencing parameters of each stage corresponding to the first control experiment with the highest shape retention rate as the optimal parameter group; Based on the change of the original powder ratio, at least one group of second control experiments of the gas pressure sintering process is carried out using the optimal parameter group to obtain each group of second ceramic samples; By performing a low-destructive test on each group of second ceramic samples, the low-destructive sample performance of each group of second ceramic samples is calculated, wherein the low-destructive sample performance is sample relative density, Vickers hardness and wear resistance; By performing a high-destructive test on each group of second ceramic samples, the high-destructive sample performance of each group of second ceramic samples is calculated, wherein the high-destructive sample performance is bending strength and fracture toughness; Based on the low-destructive sample performance and high-destructive sample performance of each group of second ceramic samples, the performance score of each group of second ceramic samples is calculated using a weight distribution formula, and the second control experiment with the highest output performance score corresponds to the original powder ratio as the optimal ratio; It is determined whether the performance score of the second ceramic sample under the optimal ratio is higher than the set score threshold. If so, no output is made; if not, the original powder ratio is reset and a third control experiment of the gas pressure sintering process is performed.

2. A parameter optimization method for the production and processing of wear-resistant ceramic glaze according to claim 1, characterized in that: The weighing of the raw powder according to the set ratio and the pretreatment of the raw materials specifically include: Set the original powder ratio and ball milling time; Pour the original powder, grinding balls and ball-milling medium anhydrous ethanol into the ball mill according to the set original powder ratio; Fix the ball mill on the turntable and perform ball milling in forward and reverse directions alternately within the set ball milling time; The ball-milled slurry is placed in an industrial drying oven and dried at 60°C until the anhydrous ethanol is basically evaporated; The dried blank is placed in a pulverizer for pulverization, and then passed through a 50-mesh and a 100-mesh sieve in turn for sieving and granulation.

3. A parameter optimization method for the production and processing of wear-resistant ceramic glaze according to claim 2, characterized in that: Based on the changes of the influencing parameters at each stage, the powder is heated, pressurized and cooled step by step by using the gas pressure sintering process, and at least one group of first control experiments is performed to obtain each group of first ceramic samples, which specifically includes: Set the influencing parameter values ​​of each stage of each group of control experiments; Introduce nitrogen into the sintering furnace to raise the pressure inside the furnace to the first stage pressure; The temperature is raised to a first insulation temperature at a first heating rate, and the insulation time is set to the first insulation time; Continue to introduce nitrogen to pressurize to the second stage pressure; The temperature is raised to a second insulation temperature at a second heating rate, and the insulation time is set to the second insulation time; The temperature is raised to a third insulation temperature at a third heating rate, and the insulation time is set to the third insulation time; Cooling the temperature to a fourth insulation temperature at a first cooling rate, and setting the insulation time to a fourth insulation time; Cooling the temperature to the fifth insulation temperature at the second cooling rate, and the insulation time is set to the fifth insulation time; The sintering furnace is cooled down naturally to room temperature, and the pressure inside the furnace is reduced to normal pressure; The furnace is opened and the first ceramic samples of each group that have been sintered are taken out.

4. A parameter optimization method for the production and processing of wear-resistant ceramic glaze according to claim 3, characterized in that: The method of calculating the shape retention rate of each group of first ceramic samples and outputting the influencing parameters of each stage corresponding to the first control experiment with the highest shape retention rate as the optimal parameter group specifically includes: Modeling each group of first ceramic samples to obtain each group of first ceramic sample models; Obtain standard ceramic models; The shape retention rate of each group of first ceramic samples is calculated using the shape retention rate formula; The influencing parameters of each stage corresponding to the first control experiment with the highest output shape retention rate are the optimal parameter groups; The shape retention rate formula includes: , In the formula, is the shape retention rate of the first ceramic sample in group i, is the overlapping volume of the first ceramic sample model and the standard ceramic model of the i-th group, is the total volume of the standard ceramic model.

5. A parameter optimization method for the production and processing of wear-resistant ceramic glaze according to claim 4, characterized in that: The method of performing a low-destructive test on each group of second ceramic samples to calculate the low-destructive sample performance of each group of second ceramic samples specifically includes: The volume density of the second ceramic sample in each group was calculated using the water displacement method; Calculating the sample relative density of each group of second ceramic samples using a relative density formula based on the volume density of each group of second ceramic samples; The second ceramic samples of each group are placed directly under the diamond indenter of the Vickers hardness tester, and the normal load and stress time are set; Take at least two different areas for hardness testing; Observe the surface indentation through an optical microscope and record the diagonal length of the corresponding indentation; Calculating the Vickers hardness of each group of second ceramic samples using a Vickers hardness calculation formula; Silicon nitride ceramic balls are used as friction devices; Set the friction normal load, sliding frequency, friction stroke and friction time; Conducting friction test on at least one location of each group of second ceramic samples by dry sliding reciprocating friction method; measuring the friction coefficient of the surface of each group of second ceramic samples after the friction test; The wear resistance of each group of second ceramic samples is calculated using the wear resistance formula; The sample relative density, Vickers hardness and wear resistance of each group of second ceramic samples are combined and output as low-destructive sample performance of each group of second ceramic samples; The bulk density is: , In the formula, is the volume density of the second ceramic sample in the i-th group, is the mass of the second ceramic sample in the i-th group, is the mass of the second ceramic sample in group i after absorbing water, is the floating weight of the second ceramic sample in group i, is the density of distilled water; The relative density formula is: , In the formula, is the relative density of the second ceramic sample in group i, is the theoretical density of the ceramic sample; The Vickers hardness calculation formula is: , In the formula, is the Vickers hardness of the second ceramic sample in group i, To set the normal load, is the arithmetic mean of the diagonal lengths of the surface indentations of the second ceramic sample in the i-th group; The wear resistance formula is: , In the formula, is the wear resistance of the second ceramic sample in group i, is the friction coefficient of the second ceramic sample at the jth position in the i-th group, The number of friction tests performed on the second ceramic sample of the i-th group.

6. A parameter optimization method for the production and processing of wear-resistant ceramic glaze according to claim 5, characterized in that: The method of performing a high-destructive test on each group of second ceramic samples to calculate the high-destructive sample performance of each group of second ceramic samples specifically includes: Cut off a portion of each group of second ceramic samples and process them into two rectangular parallelepiped samples of set sizes; The three-point bending method is used to apply pressure to the two ends and the middle of one of the rectangular samples in each group; The maximum load just before the sample breaks is recorded as the first breaking load; Calculating the bending strength of each group of second ceramic samples using a bending strength formula; The single-edge notched beam method was used to make a small notch in the middle of one of the rectangular samples in each group as a pre-set crack; Apply pressure to both ends of the rectangular sample and record the maximum load just before the sample breaks as the second breaking load; The fracture toughness of each group of second ceramic samples is calculated using the fracture toughness formula; The bending strength and fracture toughness of each group of second ceramic samples are combined and output as high destructive sample properties of each group of second ceramic samples; The bending strength formula is: , In the formula, is the flexural strength of the second ceramic sample in group i, is the first fracture load of the second ceramic sample in the i-th group, is the length of the cuboid sample, is the height of the cuboid sample, is the width of the rectangular sample; The fracture toughness formula is: , In the formula, is the fracture toughness of the second ceramic sample in group i, is the second fracture load of the second ceramic sample in group i, is the incision length.

7. A parameter optimization method for the production and processing of wear-resistant ceramic glaze according to claim 6, characterized in that: The method of calculating the performance scores of the second ceramic samples of each group based on the low-destructive sample performance and the high-destructive sample performance of each group of the second ceramic samples by using a weight distribution formula and outputting the second control experiment with the highest performance score as the optimal ratio of the original powder material specifically includes: Obtaining the score weights of each low-destructive sample performance and high-destructive sample performance; Calculate the performance score of each group of second ceramic samples using a weight distribution formula based on the score weight; The second control experiment with the highest output performance score corresponds to the optimal ratio of original powder material; The weight distribution formula is: , In the formula, is the performance score of the second ceramic sample in group i, , , , , They are the score weights of sample relative density, Vickers hardness, wear resistance, bending strength and fracture toughness respectively.

8. A parameter optimization method for the production and processing of wear-resistant ceramic glaze according to claim 7, characterized in that: The step of judging whether the performance score of the second ceramic sample at the optimal ratio is higher than the set score threshold specifically includes: Obtaining a performance score of the second ceramic sample at the optimal ratio; Set scoring thresholds; It is determined whether the performance score of the second ceramic sample under the optimal ratio is higher than the set score threshold. If so, no output is made; if not, the original powder ratio is reset and a third control experiment of the gas pressure sintering process is performed.