Modified gamma-polyglutamic acid hemostatic gel material as well as preparation method and application thereof
Through the amidation cross-linking of dopamine-modified γ-polyglutamic acid and gelatin and tannic acid hydrogen bonding cross-linking, a double-cross-linked hydrogel was prepared, which solved the inconvenience and inconvenience of using existing hemostatic materials in emergency hemostasis scenarios. It solves the problem of incompatibility and achieves a fast and safe hemostasis effect, and is suitable for a variety of emergency situations.
Patent Information
- Application Number
- CN202410584520.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-12
- Publication Date
- 2024-09-27
AI Technical Summary
Existing hemostatic materials have problems such as inconvenience, high cost, unsuitability for different patient groups and may cause burns in emergency hemostasis scenarios, and cannot quickly and effectively control acute massive bleeding.
Dopamine-modified γ-polyglutamic acid is cross-linked with gelatin through amidation reaction, and the polyphenolic structure of tannic acid is used to form hydrogen bond cross-linking with gelatin to prepare a double-crosslinked hydrogel to form a highly water-absorbent hydrogel. , Highly adhesive modified γ-polyglutamic acid hemostatic gel material.
It achieves rapid hemostasis, is safe and non-toxic, and can quickly heal wounds. It is suitable for accidents, battlefield first aid and surgical operations. The material stability and biocompatibility are improved, and it can be widely used in different patient groups.
Smart Images

Figure CN118697929A
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of medical materials, and in particular relates to a modified gamma-polyglutamic acid hemostatic gel material and a preparation method and application thereof. Background Art
[0002] In scenarios such as accidents and surgical operations, achieving rapid and effective hemostasis is of great significance. There are many types of hemostatic materials currently on the market, including gauze, hemostatic bandages, gelatin sponges, fibrin sealants, HemCon chitosan dressings, QuickClot, etc. However, these materials still have some shortcomings, which limit their application in emergency hemostasis scenarios. For example, gauze and hemostatic bandages can only provide temporary compression hemostasis, while gelatin sponges are only suitable for treating wound bleeding and cannot meet the needs of acute massive bleeding. Although fibrin sealants perform well in hemostatic effects, they are expensive and need to be thawed in advance, which is cumbersome to operate. HemCon chitosan dressings are not suitable for patients with shellfish allergies, and their hemostatic effects are highly dependent on their physical and chemical properties, including deacetylation degree, molecular weight, viscosity, etc. As for QuickClot, although it is an FDA-approved hemostatic agent composed of zeolite, it releases a lot of heat when absorbing liquids, which may cause burns to patients. Therefore, there is an urgent need to develop a new hemostatic material that can quickly block acute massive bleeding, has good biocompatibility, and is easy to use. This material should be able to be quickly applied at the first aid site or during surgery to effectively control bleeding and promote wound healing, thereby reducing the risk of serious complications caused by blood loss in patients. At the same time, the material should also have the characteristics of reasonable cost, simple operation, and wide applicability to different patient groups to ensure that it can provide reliable hemostatic effects in various emergency situations.
[0003] In this application context, the inventors of the present invention provide a new modified γ-polyglutamic acid hemostatic gel material. Summary of the invention
[0004] The first technical problem solved by the present invention is to provide a new modified gamma-polyglutamic acid hemostatic gel material which can quickly stop bleeding.
[0005] The modified gamma-polyglutamic acid hemostatic gel material of the invention is a double cross-linked hydrogel product prepared by cross-linking dopamine-modified gamma-polyglutamic acid and gelatin through amidation reaction and forming hydrogen bonds with gelatin through the polyphenol structure of tannic acid.
[0006] Wherein, the structural formula of dopamine-modified γ-polyglutamic acid (γ-PGA-DA) is shown in Formula I:
[0007]
[0008] Among them, R1 is n is a natural number greater than 1000 and less than 10000; the percentage of R1 to the total number of carboxyl groups on the chain is 1 to 50%.
[0009] The R1H described in the present invention is dopamine.
[0010] The dopamine-modified γ-polyglutamic acid of the present invention is prepared by the following method:
[0011] (1) γ-polyglutamic acid is dissolved in deionized water, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide are added to activate the γ-polyglutamic acid;
[0012] (2) adding R1H to the mixture obtained in step (1), adjusting the pH to 5-6, and reacting under nitrogen atmosphere in a dark environment to obtain a reaction product;
[0013] (3) The reaction product obtained in step (2) is dialyzed using a dialysis bag with Mw=8000-12000 at room temperature, and dried to obtain dopamine-modified γ-polyglutamic acid.
[0014] In the preparation method of the above dopamine-modified γ-polyglutamic acid:
[0015] The molecular weight of the γ-polyglutamic acid in step (1) is 100,000 to 2,000,000.
[0016] In the step (1), γ-polyglutamic acid is dissolved in deionized water until the concentration of γ-polyglutamic acid is 10 to 100 g / L.
[0017] In the step (1), the molar ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride to γ-polyglutamic acid monomer is 1 to 2:1.
[0018] The molar ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride to N-hydroxysuccinimide in step (1) is 2 to 4:1.
[0019] In the step (2), the molar ratio of dopamine to γ-polyglutamic acid monomer is 2-4:1.
[0020] Furthermore, the addition amounts of the above four components are calculated according to the molar ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide, dopamine, and γ-polyglutamic acid monomer: 1-2:0.5:2-4:1.
[0021] The activation time in step (1) is 20 to 40 minutes.
[0022] Preferably, the activation time in step (1) is 30 minutes.
[0023] The reaction time under nitrogen conditions in step (2) is 12 to 48 hours.
[0024] Preferably, the reaction time under nitrogen conditions in step (2) is 24 hours.
[0025] The dialysis time in step (3) is 48 to 120 hours.
[0026] Preferably, the dialysis time in step (3) is 96 hours.
[0027] The drying in step (3) is freeze-drying.
[0028] The second technical problem solved by the present invention is to provide a method for preparing the modified γ-polyglutamic acid hemostatic gel material of the present invention, comprising the following steps:
[0029] A. Dissolve tannic acid in deionized water, add dopamine-modified γ-polyglutamic acid, and mix until dissolved to obtain a modified γ-polyglutamic acid / tannic acid mixed solution;
[0030] B. Dissolve gelatin in deionized water, add the modified γ-polyglutamic acid / tannic acid mixed solution obtained in step A, and mix to obtain a modified γ-polyglutamic acid / gelatin / tannic acid mixed solution;
[0031] C. Adding the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained in step B into a coagulation bath, wherein the pH value of the coagulation bath is 5 to 6, and reacting at a temperature of 40 to 50° C. to obtain a cross-linked modified γ-polyglutamic acid / gelatin / tannic acid hydrogel;
[0032] D. The modified γ-polyglutamic acid / gelatin / tannic acid hydrogel obtained in step C is freeze-dried, cut or crushed into blocks or powders to obtain the modified γ-polyglutamic acid hemostatic gel material.
[0033] In the preparation method of the modified γ-polyglutamic acid hemostatic gel material:
[0034] In the step A, the mass concentration of tannic acid in the solution obtained by dissolving tannic acid in deionized water is 0.5-4%.
[0035] Preferably, in step A, the mass concentration of tannic acid in the solution obtained by dissolving tannic acid in deionized water is 0.5-2%.
[0036] Most preferably, the mass concentration of tannic acid in the solution obtained by dissolving tannic acid in deionized water in step A is 1-2%.
[0037] The mass concentration of dopamine-modified γ-polyglutamic acid in the solution obtained by adding dopamine-modified γ-polyglutamic acid in step A is 10-30%.
[0038] Preferably, the mass concentration of dopamine-modified γ-polyglutamic acid in the solution obtained by adding dopamine-modified γ-polyglutamic acid in step A is 30%.
[0039] The mixing in step A is carried out by continuous stirring, so as to completely dissolve the dopamine-modified γ-polyglutamic acid.
[0040] In the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution in step B, the mass ratio of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin is 0.5-2:10-30:8-15.
[0041] Preferably, the mass ratio of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution in step B is 0.5 to 2:30:15.
[0042] Most preferably, the mass ratio of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixture in step B is 1-2:30:15.
[0043] The total mass concentration of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained in step B is 15-30%.
[0044] Preferably, the total mass concentration of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained in step B is 20-25%.
[0045] Most preferably, the total mass concentration of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained in step B is 22-24%.
[0046] In the step B, gelatin is dissolved in deionized water at a temperature of 40 to 50° C. and stirred slowly until the gelatin is completely dissolved.
[0047] Preferably, in step B, gelatin is dissolved in deionized water at 45° C. and stirred slowly until the gelatin is completely dissolved.
[0048] The mixing in step B is carried out by rapid stirring at a temperature of 40 to 50° C. until the mixture is uniformly stirred.
[0049] Preferably, the mixing in step B is performed by rapid stirring at a temperature of 45° C. until the mixture is uniformly stirred.
[0050] The mixing and stirring time in step B is 0.5 to 2 hours.
[0051] Preferably, the stirring time of mixing in step B is 1 hour.
[0052] The modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained by mixing in step B is then subjected to a degassing treatment.
[0053] In the step C, the concentration of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride in the coagulation bath is 2.5-5 g / L, the concentration of N-hydroxysuccinimide is 1-2.5 g / L, and the solvent is deionized water.
[0054] Preferably, in the coagulation bath in step C, the concentration of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride is 5 g / L, the concentration of N-hydroxysuccinimide is 2.5 g / L, and the solvent is deionized water.
[0055] The temperature condition in step C is 0°C.
[0056] The reaction time in step C is 20 to 60 minutes.
[0057] Preferably, the reaction time in step C is 30 min.
[0058] The volume ratio of the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution to the coagulation bath in step C is (5-15):100.
[0059] Preferably, in step C, the volume ratio of the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution to the coagulation bath is 10:100.
[0060] The freeze drying condition in the step D is freeze drying at a temperature of -60 to -40°C.
[0061] Preferably, the freeze-drying condition in step D is freeze-drying at a temperature of -50°C.
[0062] The freeze-drying time in step D is 48 to 120 hours.
[0063] Preferably, the freeze-drying time condition in step D is 96 hours.
[0064] The gel in step D is freeze-dried to form a sponge-like product, and the pulverization can be cut or pulverized to obtain a sponge block or powder, thus obtaining the modified γ-polyglutamic acid hemostatic gel material of the present invention.
[0065] The third technical problem solved by the present invention is to provide the use of the modified γ-polyglutamic acid hemostatic gel material of the present invention in the preparation of a hemostatic agent.
[0066] The modified γ-polyglutamic acid hemostatic gel material of the present invention is a highly water-absorbent and highly adhesive rapid hemostatic material, and the material forms include sponge block and powder. The modified γ-polyglutamic acid hemostatic gel material of the present invention adopts dopamine to modify γ-polyglutamic acid, and the dopamine modification improves the performance of γ-polyglutamic acid, enhances the stability and biocompatibility of the material; then cross-links with gelatin through an amidation reaction, and then cross-links to form a gel through the hydrogen bond between the polyphenol structure of tannic acid and gelatin, and a double cross-linking method forms a tight network structure, and the double cross-linking network can enhance the mechanical properties of the hemostatic material, and can prevent the hemostatic material from dissolving quickly after absorbing water, and the high water absorption of γ-polyglutamic acid can enhance the hemostatic performance of the hemostatic material. In addition, after the hemostatic material encounters a wound site, the dopamine group on the modified γ-polyglutamic acid chain and the tannic acid can be complexed and cross-linked with the wound tissue, and has good adhesion. The gel can fit closely with the wound when used, thereby forming a stable blood clot at the bleeding wound, and achieving a faster hemostatic effect. Compared with traditional hemostatic materials, the modified γ-polyglutamic acid hemostatic gel material provided by the present invention has the advantages of fast hemostasis, safety and non-toxicity, and rapid wound healing. In addition, the preparation method is simple and efficient, and can be applied to scenarios such as accidents, battlefield first aid and surgical hemostasis. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] Figure 1 Polyglutamic acid (γ-PGA) and dopamine-modified γ-polyglutamic acid (γ-PGA-DA) 1 HNMR spectrum.
[0068] Figure 2 UV absorption spectra of polyglutamic acid (γ-PGA) and dopamine-modified γ-polyglutamic acid (γ-PGA-DA).
[0069] Figure 3 This is a graph showing the hemolytic performance of the modified γ-polyglutamic acid hemostatic gel material prepared in Example 1-4.
[0070] Figure 4 The figure shows the hemostatic process of the modified γ-polyglutamic acid hemostatic gel material prepared in Example 3 in the rat femoral artery anticoagulation hemostasis model.
[0071] Figure 5 The figure shows the hemostatic process of the modified γ-polyglutamic acid hemostatic gel material prepared in Example 3 in the rabbit femoral artery anticoagulation hemostasis model.
[0072] Figure 6 This is the hemostatic process of the modified γ-polyglutamic acid hemostatic gel material prepared in Example 3 in the rabbit liver anticoagulation hemostasis model. DETAILED DESCRIPTION
[0073] Below in conjunction with embodiment, the scheme of the present invention will be explained and described.It will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be regarded as limiting the scope of the present invention.In the embodiment, if no specific technology or condition is indicated, it is carried out according to the technology or condition described in the document in this area or according to the product specification.The reagents used or the instruments that do not indicate the manufacturer are all conventional products that can be obtained by commercial purchase.
[0074] The modified γ-polyglutamic acid hemostatic gel material of the present invention is a double cross-linked hydrogel product prepared by cross-linking dopamine-modified γ-polyglutamic acid with gelatin through amidation reaction, and forming hydrogen bonds with gelatin using the polyphenol structure of tannic acid. The structural formula of dopamine-modified γ-polyglutamic acid (γ-PGA-DA) is shown in Formula I:
[0075]
[0076] Among them, R1 is n is a natural number greater than 1000 and less than 10000; the percentage of R1 to the total number of carboxyl groups on the chain is 1 to 50%.
[0077] The R1H described in the present invention is dopamine.
[0078] The dopamine-modified γ-polyglutamic acid of the present invention is prepared by the following method:
[0079] (1) γ-polyglutamic acid is dissolved in deionized water, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide are added to activate the γ-polyglutamic acid;
[0080] (2) adding R1H to the mixture obtained in step (1), adjusting the pH to 5-6, and reacting under nitrogen atmosphere in a dark environment to obtain a reaction product;
[0081] (3) The reaction product obtained in step (2) is dialyzed using a dialysis bag with Mw=8000-12000 at room temperature, and dried to obtain dopamine-modified γ-polyglutamic acid.
[0082] In the preparation method of the above dopamine-modified γ-polyglutamic acid:
[0083] The molecular weight of the γ-polyglutamic acid in step (1) is 100,000 to 2,000,000;
[0084] In the step (1), γ-polyglutamic acid is dissolved in deionized water until the concentration of γ-polyglutamic acid is 10 to 100 g / L.
[0085] In the step (1), the molar ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride to γ-polyglutamic acid monomer is 1 to 2:1.
[0086] The molar ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride to N-hydroxysuccinimide in step (1) is 2 to 4:1.
[0087] In the step (2), the molar ratio of dopamine to γ-polyglutamic acid monomer is 2-4:1.
[0088] Furthermore, the addition amounts of the above four components are calculated according to the molar ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide, dopamine, and γ-polyglutamic acid monomer: 1-2:0.5:2-4:1.
[0089] The activation time in step (1) is 20 to 40 minutes.
[0090] Preferably, the activation time in step (1) is 30 minutes.
[0091] The reaction time under nitrogen conditions in step (2) is 12 to 48 hours.
[0092] Preferably, the reaction time under nitrogen conditions in step (2) is 24 hours.
[0093] The dialysis time in step (3) is 48 to 120 hours.
[0094] Preferably, the dialysis time in step (3) is 96 hours.
[0095] The drying in step (3) is freeze-drying.
[0096] The preparation method of the modified γ-polyglutamic acid hemostatic gel material of the present invention comprises the following steps:
[0097] A. Dissolve tannic acid in deionized water, add dopamine-modified γ-polyglutamic acid, and mix until dissolved to obtain a modified γ-polyglutamic acid / tannic acid mixed solution;
[0098] B. Dissolve gelatin in deionized water, add the modified γ-polyglutamic acid / tannic acid mixed solution obtained in step A, and mix to obtain a modified γ-polyglutamic acid / gelatin / tannic acid mixed solution;
[0099] C. Adding the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained in step B into a coagulation bath, wherein the pH value of the coagulation bath is 5 to 6, and reacting at a temperature of 40 to 50° C. to obtain a cross-linked modified γ-polyglutamic acid / gelatin / tannic acid hydrogel;
[0100] D. The modified γ-polyglutamic acid / gelatin / tannic acid hydrogel obtained in step C is freeze-dried, cut or crushed into blocks or powders to obtain the modified γ-polyglutamic acid hemostatic gel material.
[0101] In the preparation method of the modified γ-polyglutamic acid hemostatic gel material:
[0102] In the step A, the mass concentration of tannic acid in the solution obtained by dissolving tannic acid in deionized water is 0.5-4%.
[0103] Preferably, in step A, the mass concentration of tannic acid in the solution obtained by dissolving tannic acid in deionized water is 0.5-2%.
[0104] Most preferably, the mass concentration of tannic acid in the solution obtained by dissolving tannic acid in deionized water in step A is 1-2%.
[0105] The mass concentration of dopamine-modified γ-polyglutamic acid in the solution obtained by adding dopamine-modified γ-polyglutamic acid in step A is 10-30%.
[0106] Preferably, the mass concentration of dopamine-modified γ-polyglutamic acid in the solution obtained by adding dopamine-modified γ-polyglutamic acid in step A is 30%.
[0107] The mixing in step A is carried out by continuous stirring, so as to completely dissolve the dopamine-modified γ-polyglutamic acid.
[0108] In the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution in step B, the mass ratio of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin is 0.5-2:10-30:8-15.
[0109] Preferably, the mass ratio of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution in step B is 0.5 to 2:30:15.
[0110] Most preferably, the mass ratio of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixture in step B is 1-2:30:15.
[0111] The total mass concentration of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained in step B is 15-30%.
[0112] Preferably, the total mass concentration of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained in step B is 20-25%.
[0113] Most preferably, the total mass concentration of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained in step B is 22-24%.
[0114] In the step B, gelatin is dissolved in deionized water at a temperature of 40 to 50° C. and stirred slowly until the gelatin is completely dissolved.
[0115] Preferably, in step B, gelatin is dissolved in deionized water at 45° C. and stirred slowly until the gelatin is completely dissolved.
[0116] The mixing in step B is carried out by rapid stirring at a temperature of 40 to 50° C. until the mixture is uniformly stirred.
[0117] Preferably, the mixing in step B is performed by rapid stirring at a temperature of 45° C. until the mixture is uniformly stirred.
[0118] The mixing and stirring time in step B is 0.5 to 2 hours.
[0119] Preferably, the stirring time of mixing in step B is 1 hour.
[0120] The modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained by mixing in step B is then subjected to a degassing treatment.
[0121] In the step C, the concentration of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride in the coagulation bath is 2.5-5 g / L, the concentration of N-hydroxysuccinimide is 1-2.5 g / L, and the solvent is deionized water.
[0122] Preferably, in the coagulation bath in step C, the concentration of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride is 5 g / L, the concentration of N-hydroxysuccinimide is 2.5 g / L, and the solvent is deionized water.
[0123] The temperature condition in step C is 0°C.
[0124] The reaction time in step C is 20 to 60 minutes.
[0125] Preferably, the reaction time in step C is 30 min.
[0126] The volume ratio of the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution to the coagulation bath in step C is (5-15):100.
[0127] Preferably, in step C, the volume ratio of the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution to the coagulation bath is 10:100.
[0128] The freeze drying condition in the step D is freeze drying at a temperature of -60 to -40°C.
[0129] Preferably, the freeze-drying condition in step D is freeze-drying at a temperature of -50°C.
[0130] The freeze-drying time in step D is 48 to 120 hours.
[0131] Preferably, the freeze-drying time condition in step D is 96 hours.
[0132] The gel in step D is freeze-dried to form a sponge-like product, and the pulverization can be cut or pulverized to obtain a sponge block or powder, thus obtaining the modified γ-polyglutamic acid hemostatic gel material of the present invention.
[0133] In the embodiments of the hemostasis experiment of the present invention, the rats used were purchased from Chengdu Dashuo Experimental Animal Co., Ltd. γ-polyglutamic acid (γ-PGA) was purchased from Xi'an Hengji Chemical Co., Ltd. Dopamine hydrochloride, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide, and Na2HPO4 were purchased from Shanghai Aladdin Industrial Co., Ltd. Gelatin and tannic acid were purchased from Shanghai McLean Company.
[0134] The preparation method of dopamine-modified γ-polyglutamic acid used in this experiment is as follows:
[0135] Dissolve 10g of γ-polyglutamic acid with a molecular weight of 2 million in 100mL of deionized water, then add 10g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 6g of N-hydroxysuccinimide to activate γ-polyglutamic acid for 30min, then add 12g of dopamine hydrochloride, use Na2HPO4 to adjust the pH of the reaction solution to 5-6, react for 24h at room temperature in the absence of light and nitrogen, then dialyze the reaction product at room temperature with a dialysis bag of Mw=8000-12000 for 96h, and freeze-dry to obtain γ-polyglutamic acid modified by dopamine. The NMR images of γ-polyglutamic acid (γ-PGA) and dopamine-modified γ-polyglutamic acid (γ-PGA-DA) are shown in Figure 1 , UV absorption spectrum see Figure 2 .
[0136] The dopamine-modified γ-polyglutamic acid prepared by the above method is used for preparing the following modified γ-polyglutamic acid hemostatic gel material:
[0137] Example 1 Preparation of modified γ-polyglutamic acid hemostatic gel material
[0138] Dissolve 0.025g of tannic acid in 10mL of deionized water, then add 3g of dopamine-modified γ-polyglutamic acid to the deionized water, and continue stirring until completely dissolved to obtain a modified γ-polyglutamic acid / tannic acid mixture. Then, dissolve 1.5g of gelatin in 10mL of deionized water, slowly stir at 45°C until the gelatin is completely dissolved, then add 10mL of the modified γ-polyglutamic acid / tannic acid mixture, and quickly mechanically stir at 45°C for 1h to obtain a modified γ-polyglutamic acid / gelatin / tannic acid mixture and eliminate bubbles. 20 mL of the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution was extruded into a 200 mL deionized water coagulation bath containing 1 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.5 g of N-hydroxysuccinimide, and the pH of the coagulation bath was adjusted to 5-6 using Na2HPO4. The mixture was reacted at 0°C for 30 min, and then the cross-linked modified γ-polyglutamic acid / gelatin / tannic acid hydrogel was freeze-dried at -50°C for 48 h. After being crushed into powder using a grinder, a powdered modified γ-polyglutamic acid hemostatic gel material was obtained.
[0139] Example 2 Preparation of modified γ-polyglutamic acid hemostatic gel material
[0140] Dissolve 0.05g of tannic acid in 10mL of deionized water, then add 3g of dopamine-modified γ-polyglutamic acid to the deionized water and continue stirring until completely dissolved. Then, dissolve 1.5g of gelatin in 10mL of deionized water and stir at 45°C until the gelatin is completely dissolved, then add 10mL of modified γ-polyglutamic acid / tannic acid mixture and stir rapidly at 45°C for 1h to obtain a modified γ-polyglutamic acid / gelatin / tannic acid mixture and eliminate bubbles. 20 mL of the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution was extruded into a 200 mL deionized water coagulation bath containing 1 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.5 g of N-hydroxysuccinimide, and the pH of the coagulation bath was adjusted to 5-6 using Na2HPO4. The mixture was reacted at 0°C for 30 min, and then the cross-linked modified γ-polyglutamic acid / gelatin / tannic acid hydrogel was freeze-dried at -50°C for 48 h. After being crushed into powder using a grinder, a powdered modified γ-polyglutamic acid hemostatic gel material was obtained.
[0141] Example 3 Preparation of modified γ-polyglutamic acid hemostatic gel material
[0142] Dissolve 0.1g of tannic acid in 10mL of deionized water, then add 3g of dopamine-modified γ-polyglutamic acid to the deionized water, and continue stirring until completely dissolved to obtain a modified γ-polyglutamic acid / tannic acid mixture. Then, dissolve 1.5g of gelatin in 10mL of deionized water, slowly stir at 45°C until the gelatin is completely dissolved, then add 10mL of the modified γ-polyglutamic acid / tannic acid mixture, and quickly mechanically stir at 45°C for 1h to obtain a modified γ-polyglutamic acid / gelatin / tannic acid mixture and eliminate bubbles. 20 mL of the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution was extruded into a 200 mL deionized water coagulation bath containing 1 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.5 g of N-hydroxysuccinimide, the pH of the coagulation bath was adjusted to 5-6 using Na2HPO4, and the mixture was reacted at 0°C for 30 min. The cross-linked modified γ-polyglutamic acid / gelatin / tannic acid hydrogel was then freeze-dried at -50°C for 48 h, and crushed into powder using a grinder to obtain a powdered modified γ-polyglutamic acid hemostatic gel material.
[0143] Example 4 Preparation of modified γ-polyglutamic acid hemostatic gel material
[0144] Dissolve 0.2g of tannic acid in 10mL of deionized water, then add 3g of dopamine-modified γ-polyglutamic acid to the deionized water, and continue stirring until completely dissolved to obtain a modified γ-polyglutamic acid / tannic acid mixture. Then, dissolve 1.5g of gelatin in 10mL of deionized water, slowly stir at 45°C until the gelatin is completely dissolved, then add 10mL of the modified γ-polyglutamic acid / tannic acid mixture, and quickly mechanically stir at 45°C for 1h to obtain a modified γ-polyglutamic acid / gelatin / tannic acid mixture and eliminate bubbles. 20 mL of the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution was extruded into a 200 mL deionized water coagulation bath containing 1 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 0.5 g of N-hydroxysuccinimide, the pH of the coagulation bath was adjusted to 5-6 using Na2HPO4, and the mixture was reacted at 0°C for 30 min. The cross-linked modified γ-polyglutamic acid / gelatin / tannic acid hydrogel was then freeze-dried at -50°C for 48 h, and crushed into powder using a grinder to obtain a powdered modified γ-polyglutamic acid hemostatic gel material.
[0145] The beneficial effects of the modified γ-polyglutamic acid hemostatic gel material of the present invention were verified by hemolysis experiment and hemostasis experiment.
[0146] 1. Hemolysis test
[0147] The modified γ-polyglutamic acid hemostatic gel materials prepared in Examples 1 to 4 of the present invention were taken at appropriate weights for hemolysis experiments:
[0148] Red blood cells were collected from fresh rabbit blood, centrifuged at 3000rpm for 10 minutes, and then washed three times with normal saline. A normal saline solution containing 2% red blood cells was prepared for use. After the red blood cells were incubated with different samples at 37°C for 1 hour, the mixed solution was centrifuged. The absorbance of the supernatant at 545nm was measured using a UV spectrophotometer. Normal saline and deionized water were used as negative and positive controls, respectively. The formula for calculating the hemolysis rate is as follows: Hemolysis rate (%) = (As-An) / (Ap-An)
[0149] Where As, An and Ap represent the absorbance values of the sample, negative control and positive control, respectively. The hemolytic performance results of different hemostatic hydrogels are shown in Figure 3 .
[0150] 2. Hemostasis Experiment
[0151] 1. The modified γ-polyglutamic acid hemostatic gel material prepared in Examples 1 to 4 of the present invention was crushed into powder for later use, and a hemostasis model was established using SD rats. A total of 20 SD rats were randomly divided into 4 groups, with 5 rats in each group. After the rats were anesthetized, sodium heparin was intravenously injected into the rats as an anticoagulant in an amount of 2.5 to 3 mg / 250 to 300 g. The femoral artery in the abdomen of the rats was cut off, and then 0.5 g of the material was applied to the bleeding site and pressed for 2 minutes. After 2 minutes, the bleeding site of the rats was observed to see if there was any bleeding to determine whether the hemostasis was successful. Finally, the number of surviving rats in each group was observed after 24 hours, and the results are shown in Table 1.
[0152] Table 1 Hemostatic effect of anticoagulation SD rat femoral artery hemostasis model
[0153]
[0154] The test results show that the modified γ-polyglutamic acid hemostatic gel material prepared by the present invention can ensure a 24-hour survival rate of more than 60% in the femoral artery hemostasis model of anticoagulation rats, wherein the tannic acid content and the solid content of the material when preparing the modified γ-polyglutamic acid hemostatic gel material have an effect on the hemostatic stability of the material. In particular, the hemostatic effect of Example 3 is obvious, such as Figure 4 This is the anticoagulation and hemostasis process of the modified γ-polyglutamic acid hemostatic gel material prepared in Example 3 in the femoral artery of rats.
[0155] 2. The modified γ-polyglutamic acid hemostatic gel material prepared in Examples 1 to 4 of the present invention was crushed into powder for later use, and a hemostasis model was established using the femoral artery of rabbits. A total of 12 rabbits were randomly divided into 3 groups, with 4 rabbits in each group. After the rabbits were anesthetized, sodium heparin was intravenously injected into the rabbits as an anticoagulant in an amount of 2.5 to 3 mg / 250 to 300 g. The exposed rabbit liver was punctured with a 24G needle to produce bleeding, and then 0.5 g of the material was applied to the bleeding site and pressed for 2 minutes. After 2 minutes, the bleeding site of the rabbit liver was observed to see if there was any bleeding to determine whether the hemostasis was successful. Finally, the number of surviving rabbits in each group was observed after 24 hours, and the results are shown in Table 2.
[0156] Table 2 Hemostatic effect of anticoagulation rabbit femoral artery hemostasis model
[0157]
[0158] The test results show that the modified γ-polyglutamic acid hemostatic gel material prepared by the present invention can ensure a 24-hour survival rate of more than 60% in the anticoagulation rabbit liver hemostasis model, wherein the tannic acid content and the solid content of the material when preparing the modified γ-polyglutamic acid hemostatic gel material have an effect on the hemostatic stability of the material. In particular, the hemostatic effect of Example 3 is obvious, such as Figure 5 This is the anticoagulation and hemostasis process of the modified γ-polyglutamic acid hemostatic gel material prepared in Example 3 in the rabbit femoral artery.
[0159] 3. The modified γ-polyglutamic acid hemostatic gel material prepared in Examples 1 to 4 of the present invention was crushed into powder for later use, and a hemostatic model was established using rabbit livers. A total of 12 rabbits were included, 4 rabbits in each group, and they were randomly divided into 3 groups. After the rabbits were anesthetized, sodium heparin was intravenously injected into the rabbits as an anticoagulant, with a dosage of 2.5 to 3 mg / 250 to 300 g. The femoral artery of the rabbit was exposed and punctured with a 24G needle to produce bleeding. Subsequently, 0.5 g of the material was applied to the bleeding site and pressed for 2 minutes. After 2 minutes, the bleeding site of the rabbit liver was observed to see if there was any bleeding to determine whether the hemostasis was successful. Finally, the number of surviving rabbits in each group was observed after 24 hours, and the results are shown in Table 3.
[0160] Table 3 Hemostatic effect of anticoagulation rabbit liver hemostasis model
[0161]
[0162] The test results show that the modified γ-polyglutamic acid hemostatic gel material prepared by the present invention can ensure a 24-hour survival rate of more than 60% in the anticoagulation rabbit femoral artery hemostasis model, wherein the tannic acid content and the solid content of the material when preparing the modified γ-polyglutamic acid hemostatic gel material have an effect on the hemostatic stability of the material. In particular, the hemostatic effect of Example 3 is obvious, such as Figure 6This is the anticoagulation and hemostasis process of the modified γ-polyglutamic acid hemostatic gel material prepared in Example 3 in rabbit liver.
[0163] In summary, the preparation method of the modified γ-polyglutamic acid hemostatic gel material of the present invention is not only simple and efficient, but also the obtained gel hemostatic material has multiple advantages. The dopamine modification in the material improves the performance of γ-polyglutamic acid and enhances the stability and biocompatibility of the material. Secondly, through the double cross-linking method, a tight network structure is formed, so that the gel can better adhere to the wound surface when used, achieving a faster hemostatic effect.
Claims
1. Modified γ-polyglutamic acid hemostatic gel material, characterized in that: The double cross-linked hydrogel product is prepared by cross-linking dopamine-modified γ-polyglutamic acid with gelatin through amidation reaction, and forming hydrogen bonds with gelatin using the polyphenol structure of tannic acid. Wherein, the structural formula of dopamine-modified γ-polyglutamic acid is shown in Formula I: Among them, R1 is n is a natural number greater than 1000 and less than 10000; the percentage of R1 to the total number of carboxyl groups on the chain is 1 to 50%.
2. The modified γ-polyglutamic acid hemostatic gel material according to claim 1, characterized in that: The dopamine-modified γ-polyglutamic acid is prepared by the following method: (1) γ-polyglutamic acid is dissolved in deionized water, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide are added to activate the γ-polyglutamic acid; (2) adding dopamine to the product obtained in step (1), adjusting the pH to 5-6, and reacting under nitrogen gas in a dark environment to obtain a reaction product; (3) The reaction product obtained in step (2) is dialyzed using a dialysis bag with Mw=8000-12000 at room temperature, and dried to obtain dopamine-modified γ-polyglutamic acid.
3. The modified γ-polyglutamic acid hemostatic gel material according to claim 2, characterized in that: The preparation method of the dopamine-modified γ-polyglutamic acid satisfies at least any one of the following conditions: The molecular weight of the γ-polyglutamic acid in step (1) is 100,000 to 2,000,000; In the step (1), γ-polyglutamic acid is dissolved in deionized water until the concentration of γ-polyglutamic acid is 10 to 100 g / L; In the step (1), the molar ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride to γ-polyglutamic acid monomer is 1 to 2:1; The molar ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride to N-hydroxysuccinimide in step (1) is 2 to 4:1; In the step (2), the molar ratio of dopamine to γ-polyglutamic acid monomer is 2 to 4:1; Furthermore, the addition amount of the above four components is calculated according to the molar ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide, dopamine, and γ-polyglutamic acid monomer: 1-2﹕0.5﹕2-4﹕1; The activation time in step (1) is 20 to 40 minutes; Preferably, the activation time in step (1) is 30 min; The reaction time under nitrogen conditions in step (2) is 12 to 48 hours; Preferably, the reaction time under nitrogen conditions in step (2) is 24 hours; The dialysis time in step (3) is 48 to 120 hours; Preferably, the dialysis time in step (3) is 96 hours; The drying in step (3) is freeze-drying.
4. The method for preparing the modified γ-polyglutamic acid hemostatic gel material according to any one of claims 1 to 3, characterized in that: The steps include: A. Dissolve tannic acid in deionized water, add dopamine-modified γ-polyglutamic acid, and mix until dissolved to obtain a modified γ-polyglutamic acid / tannic acid mixed solution; B. Dissolve gelatin in deionized water, add the modified γ-polyglutamic acid / tannic acid mixed solution obtained in step A, and mix to obtain a modified γ-polyglutamic acid / gelatin / tannic acid mixed solution; C. Add the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained in step B into a coagulation bath, wherein the pH of the coagulation bath is 5 to 6, and react at a temperature of 0 to 4° C. to obtain a cross-linked modified γ-polyglutamic acid / gelatin / tannic acid hydrogel; D. The modified γ-polyglutamic acid / gelatin / tannic acid hydrogel obtained in step C is freeze-dried, cut or crushed into blocks or powders to obtain the modified γ-polyglutamic acid hemostatic gel material.
5. The method for preparing the modified γ-polyglutamic acid hemostatic gel material according to claim 4, characterized in that: At least one of the following is met: In the preparation method of the modified γ-polyglutamic acid hemostatic gel material: In the step A, the mass concentration of tannic acid in the solution obtained by dissolving tannic acid in deionized water is 0.5-4%; Preferably, the mass concentration of tannic acid in the solution obtained by dissolving tannic acid in deionized water in step A is 0.5-2%; Most preferably, the mass concentration of tannic acid in the solution obtained by dissolving tannic acid in deionized water in step A is 1-2%; The mass concentration of dopamine-modified γ-polyglutamic acid in the solution obtained by adding dopamine-modified γ-polyglutamic acid in step A is 10-30%; Preferably, the mass concentration of dopamine-modified γ-polyglutamic acid in the solution obtained by adding dopamine-modified γ-polyglutamic acid in step A is 30%; The mixing in step A is carried out by continuous stirring, so as to completely dissolve the dopamine-modified γ-polyglutamic acid.
6. The method for preparing the modified γ-polyglutamic acid hemostatic gel material according to claim 4, characterized in that: At least one of the following is met: In the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution in step B, the mass ratio of tannic acid, dopamine-modified γ-polyglutamic acid, and gelatin is 0.5-2:10-30:8-15; Preferably, the mass ratio of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixture in step B is 0.5-2:30:15; Most preferably, the mass ratio of tannic acid, dopamine-modified γ-polyglutamic acid, and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixture in step B is 1-2:30:15; The total mass concentration of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained in step B is 15-30%; Preferably, the total mass concentration of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained in step B is 20-25%; Most preferably, the total mass concentration of tannic acid, dopamine-modified γ-polyglutamic acid and gelatin in the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained in step B is 22-24%; In step B, gelatin is dissolved in deionized water and slowly stirred at a temperature of 40 to 50° C. until the gelatin is completely dissolved; Preferably, in step B, gelatin is dissolved in deionized water and slowly stirred at a temperature of 45° C. until the gelatin is completely dissolved; In step B, the mixing is carried out by rapid stirring at a temperature of 40 to 50° C. until the mixture is uniformly stirred; Preferably, the mixing in step B is carried out by rapid stirring at a temperature of 45° C. until the mixture is uniformly stirred; The mixing time in step B is 0.5 to 2 hours; Preferably, the mixing time in step B is 1 h; The modified γ-polyglutamic acid / gelatin / tannic acid mixed solution obtained by mixing in step B is then subjected to a degassing treatment.
7. The method for preparing the modified γ-polyglutamic acid hemostatic gel material according to claim 4, characterized in that: At least one of the following is met: In the step C, the concentration of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride in the coagulation bath is 2.5-5 g / L, the concentration of N-hydroxysuccinimide is 1-2.5 g / L, and the solvent is deionized water; preferably, the concentration of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride in the coagulation bath in the step C is 5 g / L, the concentration of N-hydroxysuccinimide is 2.5 g / L, and the solvent is deionized water; The temperature condition in step C is 0°C; The reaction time in step C is 20 to 60 minutes; Preferably, the reaction time in step C is 30 min; The volume ratio of the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution to the coagulation bath in step C is (5-15): 100; Preferably, in step C, the volume ratio of the modified γ-polyglutamic acid / gelatin / tannic acid mixed solution to the coagulation bath is 10:
100.
8. The method for preparing the modified γ-polyglutamic acid hemostatic gel material according to claim 4, characterized in that: At least one of the following is met: The freeze drying condition in step D is freeze drying at a temperature of -60 to -40°C; Preferably, the freeze-drying condition in step D is freeze-drying at a temperature of -50°C; The freeze drying time in step D is 48 to 120 hours; Preferably, the freeze-drying time in step D is 96 hours; The gel in step D is freeze-dried to form a sponge-like product, and the pulverization can be cut or pulverized to obtain a sponge block or powder, thus obtaining the modified γ-polyglutamic acid hemostatic gel material of the present invention.
9. Use of the modified γ-polyglutamic acid hemostatic gel material according to any one of claims 1 to 3 in the preparation of a hemostatic agent.
Citation Information
Cited By
Antibacterial dressing containing plant essential oil
CN119097754A
Temperature-sensitive gel for ray protection and preparation method thereof
CN122478834A