Carbon fiber tail gas adsorption filler

The IRMOFs-modified activated carbon-coated nanoporous carbon fibers prepared by electrospinning and high-temperature steam activation method solve the problem of low adsorption efficiency of existing carbon fiber tail gas adsorption packings, and achieve efficient treatment of high-concentration chlorobenzene waste gas and extend service life.

CN118698494APending Publication Date: 2024-09-27ANHUI DONGZHI GUANGXIN AGROCHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410761203.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-09-27

AI Technical Summary

Technical Problem

Existing carbon fiber exhaust gas adsorption packing materials have low adsorption efficiency, making it difficult to effectively treat high-concentration chlorobenzene waste gas, and have a short service life.

Method used

Nanoporous carbon fibers were prepared by electrospinning, and activated carbon was prepared by high-temperature steam activation. TBC and IRMOFs modified activated carbon solution were loaded onto the surface of nanoporous carbon fibers and coated to form IRMOFs modified activated carbon coated nanoporous carbon fibers.

Benefits of technology

It improves the adsorption capacity and service life of the exhaust gas adsorption packing, enhances the treatment efficiency of chlorobenzene waste gas, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118698494A
    Figure CN118698494A
Patent Text Reader

Abstract

The invention discloses a carbon fiber tail gas adsorption filler, and belongs to the technical field of carbon fiber composite materials. The filler is prepared by the following steps: preparing nano-porous carbon fibers by adopting an electrostatic spinning method, then preparing activated carbon by adopting a high-temperature water vapor activation method, loading TBC, then uniformly mixing the I RMOFs with an activated carbon solution loading the TBC, and finally coating the nano-porous carbon fibers with the I RMOFs and the activated carbon solution loading the TBC, the TBC is loaded in the activated carbon, and the I RMOFs and the activated carbon solution are mixed, so that the filler is prepared. The process is simple, and cost and time are saved. The nano-porous carbon fiber has an extremely high specific surface area, the adsorption efficiency can be improved, the influence of TBC on the pore structure of the activated carbon is small, it can be guaranteed that the excellent pore structure is not damaged, the needed styrene polymerization inhibitor can be introduced, and the method is more economical and efficient; the IRMOFs can provide a highly ordered pore structure and improve the adsorption effect of the activated carbon surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon fiber composite materials, and in particular relates to a carbon fiber tail gas adsorption filler. Background Art

[0002] Chlorobenzene is an important basic organic chemical raw material and an intermediate for dyes, medicines, and organic synthesis. However, as a typical volatile organic compound (VOCs), chlorobenzene gas can cause harm to the atmospheric environment. In recent years, the state has increasingly stringent emission standards for chlorobenzene and other toxic and harmful gases. GB31571-2015 "Petrochemical Industry Pollutant Emission Standards" stipulates that the emission limit of chlorobenzene in waste gas pollutants is 50mg / m 3 Therefore, the safe and efficient treatment of chlorobenzene waste gas has become one of the urgent problems to be solved by chemical companies.

[0003] As an environmentally friendly material, carbon fiber exhaust adsorption filler is widely used in exhaust treatment systems. With the intensification of global environmental problems, reducing exhaust emissions has become an important task. Adsorption technology is an efficient and stable exhaust treatment method, and carbon fiber exhaust adsorption filler is known for its large specific surface area, high porosity and good adsorption capacity. By adjusting the microstructure and chemical composition, carbon fiber can also achieve selective adsorption of specific harmful substances and improve the efficiency of exhaust treatment. However, after long-term use, carbon fiber may be damaged or fatigued, resulting in a decrease in adsorption capacity, which requires regular replacement or repair. In addition, although carbon fiber has a large specific surface area and porosity, its adsorption capacity is still limited, and frequent replacement or regeneration may be required for high-concentration exhaust.

[0004] The application life and adsorption effect of the existing carbon fiber exhaust gas adsorption filler have not yet reached the ideal use state, so it is necessary to develop a carbon fiber exhaust gas adsorption filler to improve the efficiency of exhaust gas adsorption. Summary of the invention

[0005] The purpose of the present invention is to provide a carbon fiber tail gas adsorption filler to solve the problem of low tail gas adsorption efficiency of the existing tail gas adsorption filler in the background technology.

[0006] A carbon fiber tail gas adsorption filler, the filler is composed of nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution; the nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution is prepared by the following steps:

[0007] S1. Add PVA (polyvinyl alcohol) to DMF (N,N′-dimethylformamide) under stirring until the mixture is uniformly mixed, and freeze-dry to obtain a DMF-PVA mixed solution;

[0008] S2. The DMF-PVA mixed solution was electrospun, condensed and refluxed, and stirred, and a 1.5 kV DC power supply and a syringe pump were used to prepare a carbon fiber film, which was pre-oxidized in a muffle furnace, and then carbonized in a tubular furnace, and then cooled to obtain a nanoporous carbon fiber;

[0009] S3. Add water and epoxy resin adhesive to the carbon powder mixture, and steam activate the activated carbon mixture at 900-1000 ℃;

[0010] S4. Add deionized water to the TBC (tert-butylcatechol) ethanol solution, mix well, add the activated carbon mixture obtained in S3, stir and impregnate at room temperature (25-30° C.), and filter to obtain the activated carbon mixture solution loaded with TBC;

[0011] S5. Adding I RMOFs to the TBC-loaded activated carbon mixture solution to obtain an I RMOFs-modified activated carbon solution;

[0012] S6. The nanoporous carbon fibers prepared in S2 are immersed in the I RMOFs modified activated carbon solution for 80-100 min, collected by centrifugation, and dried to obtain nanoporous carbon fibers coated with I RMOFs modified activated carbon.

[0013] Furthermore, the stirring speed of S1 and S2 is 200-400 / min.

[0014] Furthermore, the usage ratio of DMF and PVA in S1 is 100 mL:20 g.

[0015] Furthermore, in S2, the condensation reflux temperature is 85-95°C, the condensation reflux time is 4h, the muffle furnace heating rate is 2°C / min, the muffle furnace insulation temperature is 300°C, the muffle furnace insulation time is 2h, the tubular furnace heating rate is 2°C / min, the tubular furnace insulation temperature is 800°C, and the tubular furnace carbonization time is 3h.

[0016] Furthermore, the mass percentages of coconut shell carbon powder, fruit shell carbon powder and coal powder in the carbon powder mixture in S3 are 80-82%, 10-12% and 8-10% respectively.

[0017] Furthermore, the mass percentages of the carbon powder mixture, water and epoxy resin adhesive in S3 are 40-60%, 35-50% and 5-10% respectively.

[0018] Furthermore, the amount of water vapor in S3 is 15 kg / h, the pressure is 0.6 MPa, the water vapor temperature is 160-170° C., and the activation time is 240 min. The activated carbon prepared by the high-temperature water vapor activation method has a high specific surface area and a high mesoporosity.

[0019] Furthermore, the usage ratio of TBC, ethanol, deionized water and activated carbon in S4 is 1-4g:50mL:220mL:100g.

[0020] Furthermore, the immersion time in S4 is 4-6 hours.

[0021] Furthermore, in S4, a magnetic stirrer or a vortex stirrer is used for stirring, the stirring time is 18-30 minutes, and the stirring speed is 400-600 rpm. The purpose of stirring is to fully mix the activated carbon and water, increase the contact area, and improve the adsorption efficiency.

[0022] Furthermore, the filtration in S4 uses a filter to remove impurities in the activated carbon and water to obtain a clear activated carbon solution.

[0023] Furthermore, the dosage ratio of I RMOFs and TBC-loaded activated carbon solution in S5 is 1-2 g: 100-150 mL.

[0024] Furthermore, both the IRMOFs and the TBC-loaded activated carbon in S5 have a large number of surface active sites and the IRMOFs can provide a highly ordered pore structure, which can contact and interact with each other, thereby improving the adsorption effect of the activated carbon surface.

[0025] Furthermore, the drying in S6 uses a temperature gradient drying method with a heating rate of 5°C / min, heating from room temperature to 50°C, keeping warm for 20-25min, then heating to 80°C, keeping warm for 23-30min; gradually increasing the temperature is used to avoid generating internal stress and forming cracks.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The present invention provides a carbon fiber exhaust gas adsorption filler, which adopts an electrostatic spinning method to prepare nanoporous carbon fibers, and then adopts a high-temperature steam activation method to prepare activated carbon and load TBC, and then I RMOFs and an activated carbon solution loaded with TBC are evenly mixed, and finally coated on the nanoporous carbon fibers. The prepared I RMOFs modified activated carbon-coated nanoporous carbon fiber seat exhaust gas adsorption filler has a high efficiency exhaust gas adsorption capacity.

[0028] 2. The present invention uses nanoporous carbon fiber as a filler base material. Nanoporous carbon fiber has a large number of microscopic holes and nanoscale pore structures, which makes it have an extremely high specific surface area. The high specific surface area can provide more active sites and adsorption surfaces, thereby increasing the efficiency of applications such as catalysis, adsorption and separation.

[0029] 3. The TBC used in the present invention has little effect on the pore structure of activated carbon. The activated carbon material prepared by the room temperature impregnation method can not only ensure that the excellent pore structure is not destroyed when the TBC concentration is low, but also introduce the required styrene inhibitor. TBC is more economical and efficient than 2,6-di-tert-butyl-p-cresol (BHT).

[0030] 4. The present invention adopts a high-temperature steam activation method to prepare activated carbon, which has low production cost and large production volume. The activated carbon prepared by the high-temperature steam activation method has a high specific surface area and high mesoporosity, which can effectively improve economic benefits and enhance the adsorption effect of activated carbon.

[0031] 5. The I RMOFs used in the present invention are composed of a cubic array of Zn bridged by 6 different organic ligands. 4O (CO2) units form a three-dimensional network structure, Zn 4O The complex is alternately connected by organic ligands to form an alternating cavity structure with two different sizes. Most of these MOFs are currently used for gas adsorption and storage. Both I RMOFs and TBC-loaded activated carbon have a large number of surface active sites and I RMOFs can provide a highly ordered pore structure that can contact and interact with each other, thereby improving the adsorption effect of the activated carbon surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a flow chart of a method for preparing a carbon fiber exhaust gas adsorption filler according to an embodiment of the present application. DETAILED DESCRIPTION

[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] In the following examples and comparative examples, I RMOFs were purchased from Shanghai Kaishu Chemical Co., Ltd.

[0035] Example 1

[0036] See also Figure 1 , a carbon fiber tail gas adsorption filler, the filler is composed of nanoporous carbon fiber coated with I RMOFs modified activated carbon solution; the nanoporous carbon fiber coated with I RMOFs modified activated carbon solution is prepared as follows:

[0037] S1. Add 20 g of PVA to 100 mL of DMF under stirring at 300 rpm until the mixture is uniformly mixed, and freeze-dry to obtain a DMF-PVA mixed solution;

[0038] S2. The DMF-PVA mixed solution was subjected to electrospinning, stirred, condensed and refluxed at 90°C for 4 hours, and then prepared into a carbon fiber film using a 1.5 kV DC power supply and a syringe pump. The film was heated to 300°C at a heating rate of 2°C / min in a muffle furnace, kept warm for 2 hours for pre-oxidation, and then placed in a tubular furnace and heated to 800°C at a heating rate of 2°C / min, carbonized for 3 hours, and cooled to obtain nanoporous carbon fibers.

[0039] S3, weighing each component according to the mass percentage of 50% carbon powder mixture, 42% water and 8% epoxy resin adhesive, wherein the mass percentages of coconut shell carbon powder, fruit shell carbon powder and coal carbon powder in the carbon powder mixture are 82%, 10% and 8% respectively, adding water and epoxy resin adhesive to the carbon powder mixture, and performing steam activation at 950°C to prepare an activated carbon mixture; the steam dosage is 15kg / h, the pressure is 0.6MPa, the steam temperature is 165°C, and the activation time is 240min;

[0040] S4, add 50 mL of ethanol to 1 g of TBC, then add 220 mL of deionized water, mix well, add the activated carbon mixture obtained in S3, and immerse for 25 min at room temperature with magnetic stirring at a speed of 500 rpm, and filter to obtain an activated carbon mixture solution loaded with TBC;

[0041] S5, adding 1 g of I RMOFs to 130 mL of TBC-loaded activated carbon mixture solution to obtain an I RMOFs-modified activated carbon solution;

[0042] S6. Immerse the nanoporous carbon fibers prepared in S2 in the I RMOFs modified activated carbon solution for 90 min, collect the products by centrifugation, heat from room temperature to 50°C at a heating rate of 5°C / min, keep warm for 22 min, then heat to 80°C, keep warm for 25 min, and dry to obtain nanoporous carbon fibers coated with I RMOFs modified activated carbon.

[0043] Example 2

[0044] A carbon fiber tail gas adsorption filler, the filler is composed of nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution; the nanoporous carbon fiber coated with the I RMOFs modified activated carbon solution is prepared by the same method as in Example 1, except that the mass of TBC in S4 is 2 g, and the other components and parameters remain unchanged.

[0045] Example 3

[0046] A carbon fiber tail gas adsorption filler, the filler is composed of nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution; the preparation method of the nanoporous carbon fiber coated with the I RMOFs modified activated carbon solution is the same as that of Example 1, except that the mass of TBC in S4 is 3g, and the other components and parameters remain unchanged.

[0047] Example 4

[0048] A carbon fiber tail gas adsorption filler, the filler is composed of nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution; the preparation method of the nanoporous carbon fiber coated with the I RMOFs modified activated carbon solution is the same as that of Example 1, except that the mass of TBC in S4 is 4g, and the other components and parameters remain unchanged.

[0049] Example 5

[0050] A carbon fiber tail gas adsorption filler, the filler is composed of nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution; the nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution is prepared by the same method as in Example 1, except that the mass of I RMOFs in S5 is 2 g. The other components and parameters remain unchanged.

[0051] Example 6

[0052] A carbon fiber tail gas adsorption filler, the filler is composed of nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution; the nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution is prepared by the same method as in Example 1, except that the mass of TBC in S4 is 2 g, and the mass of I RMOFs in S5 is 2 g. The other components and parameters remain unchanged.

[0053] Example 7

[0054] A carbon fiber tail gas adsorption filler, the filler is composed of nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution; the nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution is prepared by the same method as in Example 1, except that the mass of TBC in S4 is 3g, and the mass of I RMOFs in S5 is 2g. The other components and parameters remain unchanged.

[0055] Example 8

[0056] A carbon fiber tail gas adsorption filler, the filler is composed of nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution; the nanoporous carbon fiber coated with an I RMOFs modified activated carbon solution is prepared by the same method as in Example 1, except that the mass of TBC in S4 is 4 g, and the mass of I RMOFs in S5 is 2 g. The other components and parameters remain unchanged.

[0057] Comparative Example 1

[0058] A carbon fiber tail gas adsorption filler, the preparation method of which is the same as that of Example 1, except that the activated carbon solution in S4 is not mixed with TBC, and the other components and parameters remain unchanged.

[0059] Comparative Example 2

[0060] A carbon fiber tail gas adsorption filler is prepared by the same method as in Example 1, except that in S5, I RMOFs is not used to modify the activated carbon loaded with TBC, and other components and parameters remain unchanged.

[0061] Comparative Example 3

[0062] A carbon fiber tail gas adsorption filler, the preparation method of which is the same as that of Example 1, except that a separate porous carbon fiber adsorption material is used, TBC and I RMOFs are not mixed in the activated carbon, and other components and parameters remain unchanged.

[0063] Comparative Example 4

[0064] A carbon fiber tail gas adsorption filler, the preparation method of which is the same as that of Example 1, except that the activated carbon solution in S4 is mixed with BHT, and the other components and parameters remain unchanged.

[0065] Comparative Example 5

[0066] A carbon fiber tail gas adsorption filler, the preparation method of which is the same as that of Example 1, except that in S3, a physical carbonization method is used to prepare the activated carbon, and the other components and parameters remain unchanged.

[0067] 20g of the material prepared in each implementation case was placed in a gas adsorption detection device for adsorption testing of hydrogen chloride gas, benzene vapor, and chlorobenzene vapor produced by chlorobenzene production; the initial mass concentration of the hydrogen chloride gas, benzene vapor, and chlorobenzene vapor mixed gas in the gas adsorption detection device was 250mg / m 3 After adsorption at 120°C for 1 hour, the maximum adsorption amount of different substances in the tail gas produced by chlorobenzene production was determined; the results are shown in Table 1:

[0068] Table 1

[0069] <![CDATA[Hydrogen chloride gas mg / m 3 > <![CDATA[Benzene vapor mg / m 3 > <![CDATA[Chlorobenzene vapor mg / m 3 > Example 1 127 123 122 Example 2 142 144 143 Example 3 162 165 164 Example 4 183 185 188 Example 5 143 146 146 Example 6 186 195 193 Example 7 201 204 206 Example 8 233 235 234 Comparative Example 1 105 99 101 Comparative Example 2 103 102 102 Comparative Example 3 65 63 71 Comparative Example 4 106 105 105 Comparative Example 5 113 110 109

[0070] As can be seen from Table 1, as the mass concentration of TBC loaded on the activated carbon increases and the mass of I RMOFs blended increases, the material of the present invention has a more effective adsorption effect on hydrogen chloride gas, benzene vapor, and chlorobenzene vapor produced by chlorobenzene production; as can be seen from Comparative Examples 1 and 2, the activated carbon loaded with only TBC or only blended with I RMOFs has a poor adsorption effect on hydrogen chloride gas, benzene vapor, and chlorobenzene vapor produced by chlorobenzene production; as can be seen from Comparative Example 3, conventional activated carbon without TBC loaded and blended with I RMOFs has the worst adsorption effect on hydrogen chloride gas, benzene vapor, and chlorobenzene vapor produced by chlorobenzene production; as can be seen from Comparative Example 4, the adsorption efficiency of BHT mixed in activated carbon solution is not as good as the adsorption efficiency of TBC mixed in activated carbon. As can be seen from Comparative Example 5, the adsorption efficiency of activated carbon prepared by physical carbonization activation method is not as good as that of activated carbon prepared by steam activation method.

[0071] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0072] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A carbon fiber tail gas adsorption filler, It is characterized in that The filler is composed of nanoporous carbon fibers coated with an IRMOFs modified activated carbon solution, and the nanoporous carbon fibers coated with an IRMOFs modified activated carbon solution are prepared by the following steps: S1. Add PVA to DMF under stirring until mixed evenly, and freeze-dry to obtain a DMF-PVA mixed solution; S2. After the DMF-PVA mixed solution was condensed, refluxed and stirred, it was prepared into a carbon fiber film using a 1.5 kV DC power supply and a syringe pump, pre-oxidized using a muffle furnace, and then carbonized in a tubular furnace, and then cooled to obtain nanoporous carbon fibers; S3. Add water and epoxy resin adhesive to the carbon powder mixture, and steam activate the activated carbon mixture at 900-1000 ℃; S4. Deionized water was added to the TBC ethanol solution, and after mixing, the activated carbon mixture obtained in S3 was added, and after impregnation, stirring and filtering were performed to obtain an activated carbon mixture solution loaded with TBC; S5. Add IRMOFs to the TBC-loaded activated carbon mixture solution, mix well to obtain an IRMOFs-modified activated carbon solution; S6. The nanoporous carbon fibers prepared in S2 are immersed in the IRMOFs modified activated carbon solution for 80-100 min, and the solution is collected by centrifugation and dried to obtain the nanoporous carbon fibers coated with IRMOFs modified activated carbon.

2. A carbon fiber tail gas adsorption filler according to claim 1, It is characterized in that The usage ratio of DMF and PVA in the S1 is 100 mL:20 g.

3. A carbon fiber tail gas adsorption filler according to claim 1, It is characterized in that In the S2, the condensation reflux temperature is 85-95°C, the condensation reflux time is 4h, the muffle furnace heating rate is 2°C / min, the muffle furnace insulation temperature is 300°C, the muffle furnace insulation time is 2h, the tubular furnace heating rate is 2°C / min, the tubular furnace insulation temperature is 800°C, and the tubular furnace carbonization time is 3h.

4. The carbon fiber tail gas adsorption filler according to claim 1, It is characterized in that The mass percentages of coconut shell carbon powder, fruit shell carbon powder and coal carbon powder in the carbon powder mixture in S3 are 80-82%, 10-12% and 8-10% respectively.

5. The carbon fiber tail gas adsorption filler according to claim 1, It is characterized in that The mass percentages of the carbon powder mixture, water and epoxy resin adhesive in S3 are 40-60%, 35-50% and 5-10% respectively.

6. The carbon fiber tail gas adsorption filler according to claim 1, It is characterized in that The water vapor dosage in S3 is 15 kg / h, the pressure is 0.6 MPa, the water vapor temperature is 160-170° C., and the activation time is 240 min.

7. The carbon fiber tail gas adsorption filler according to claim 1, It is characterized in that The usage ratio of TBC, ethanol, deionized water and activated carbon in S4 is 1-4g:50mL:220mL:100g.

8. The carbon fiber tail gas adsorption filler according to claim 1, It is characterized in that The immersion time in S4 is 4-6 hours.

9. The carbon fiber tail gas adsorption filler according to claim 1, It is characterized in that The dosage ratio of IRMOFs and TBC-loaded activated carbon solution in S5 is 1-2 g: 100-150 mL.

10. The carbon fiber tail gas adsorption filler according to claim 1, It is characterized in that The drying in S6 uses a temperature gradient drying method with a heating rate of 5°C / min, heating from room temperature to 50°C, keeping warm for 20-25min, and then heating to 80°C, keeping warm for 23-30min.