Lightweight anti-bomb explosion-proof composite armor for helicopter and preparation method of lightweight anti-bomb explosion-proof composite armor

Through multi-resin system and fiber mixing technology, combined with crack arrest, anti-ballistic, support, buffering and energy-absorbing layers, the problem of balancing helicopter protection and maneuverability is solved, achieving effective protection against high-speed projectiles and shock waves, and improving the performance of helicopters. Survivability and maneuverability for low-altitude operations.

CN118701296APending Publication Date: 2024-09-27SOUTHWEST TECHNICAL ENGINEERING RESEARCH INSTITUTE OF CHINA SOUTH IND GROUP
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410885404.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-09-27

AI Technical Summary

Technical Problem

Helicopters face threats from anti-aircraft machine guns and portable surface-to-air missiles in low-altitude operations. Existing anti-ballistic and anti-explosion composite armor has a difficult balance between protection capabilities and mobility, and is susceptible to aging and shedding due to shock waves and high temperatures, affecting the protective effect.

Method used

It adopts a multi-resin system of aramid fiber and carbon fiber mixed composite laminates, combined with a crack-stop layer, an elastic layer, a support layer, a buffer layer and an energy-absorbing layer. Through the combination of phenolic resin and epoxy resin, it forms a high-strength, resistant layer. A support layer with flammability and ablation resistance properties, and a buffer layer of epoxy resin and aluminum foam are used to improve the overall protection and energy absorption capabilities.

Benefits of technology

Under the condition of ensuring lightweight, it can effectively defend against high-speed armor-piercing incendiary bombs and fragmentation bombs, improve the survivability and maneuverability of helicopters, and reduce the probability of damage after being attacked. It also has excellent sound insulation and flame retardant properties to avoid structural aging. and shedding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118701296A
    Figure CN118701296A
Patent Text Reader

Abstract

The invention provides a lightweight anti-bomb explosion-proof composite armor for a helicopter, which relates to the field of armor protection and comprises a crack arrest layer (10), an anti-bomb layer (20), a support layer (30), a buffer layer (40) and an energy absorption layer (50) which are arranged in sequence, the supporting layer (30) adopts a multi-resin system aramid fiber and carbon fiber mixed composite laminated board, and comprises a first composite laminated board (31) and a second composite laminated board (32); the first composite laminated board (31) is obtained by compounding and laminating aramid fibers and carbon fibers with phenolic resin after the aramid fibers and the carbon fibers are mixed and woven, and the second composite laminated board (32) is obtained by compounding and laminating the aramid fibers and the carbon fibers with epoxy resin after the aramid fibers and the carbon fibers are mixed and woven; the buffer layer (40) is of a composite structure of epoxy resin and foamed aluminum, and the epoxy resin is located on the upper surface and the lower surface of the foamed aluminum. The composite armor can provide ballistic and explosive shock wave and fragment protection for key parts of a helicopter fuselage, and has excellent sound insulation and flame retardant properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of armor protection, and in particular to a lightweight bullet-proof and explosion-proof composite armor for a helicopter and a preparation method thereof. Background Art

[0002] In modern armed conflicts, helicopters have the characteristics of hovering in the air, being close to the ground, and not requiring a dedicated take-off and landing runway. They have greatly improved the army's mobile combat capability and have an irreplaceable special role in modern military operations. However, when helicopters are operating at medium and low altitudes, they are vulnerable to fire from the ground. In the absence of bulletproof and explosion-proof devices or insufficient protection capabilities, the risk of helicopters being hit and damaged is extremely high. At present, the protective capability of bulletproof and explosion-proof composite armor for helicopters is often closely related to weight, that is, the heavier the bulletproof and explosion-proof composite armor and the thicker it is, the stronger its protective capability; but overly heavy bulletproof and explosion-proof composite armor will seriously affect the maneuverability of the helicopter, reduce the helicopter's combat capability, and increase the probability of the helicopter being hit by fire.

[0003] For helicopters currently performing low-altitude combat missions, the main threat they face is armor-piercing incendiary bullets fired by anti-aircraft machine guns with a diameter of 12.7mm. Currently, most common helicopter protective armor is made of boron carbide and high-performance fiber-reinforced composite laminates, which are used to defend against 12.7mm armor-piercing incendiary bullets with a theoretical terminal attack speed of about 488m / s and a surface density of 44kg / m 2 , which can effectively prevent bullet penetration. However, for helicopters operating at low altitudes, there is a probability of encountering a portable surface-to-air missile attack. A strong shock wave and high-temperature combustion will be generated near the missile attack, causing a large impact on the helicopter. At the same time, local high temperatures and even burning will occur, thereby accelerating the aging and shedding of the protective armor, causing the protective armor to lose its protective function. If the protective armor's anti-ablation and anti-impact capabilities are to be improved, the thickness and weight of the protective armor must be increased, reducing the helicopter's maneuverability. In summary, there is a contradiction between the helicopter's protection capability and maneuverability, and the existing technology cannot effectively balance the relationship between the helicopter's anti-ballistic protection capability and maneuverability. Summary of the invention

[0004] In view of the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a lightweight bullet-proof and explosion-proof composite armor for helicopters, which provides protection for key parts of the helicopter fuselage against light weapons ballistics, explosion shock waves and fragments, and also has excellent sound insulation and flame retardant properties, effectively improving the survivability of the helicopter during low-altitude combat.

[0005] Another object of the present invention is to provide a method for preparing lightweight bullet-resistant and explosion-proof composite armor for helicopters.

[0006] The purpose of the present invention is achieved through the following technical solutions: A lightweight bullet-proof and explosion-proof composite armor for helicopters, comprising a crack-stop layer, an anti-bullet layer, a support layer, a buffer layer and an energy-absorbing layer which are arranged in sequence; the support layer adopts a composite laminate of aramid fiber and carbon fiber mixed with a multi-resin system, comprising a first composite laminate and a second composite laminate; the first composite laminate is close to the anti-bullet layer, and is obtained by mixing aramid fiber and carbon fiber and then laminating them with phenolic resin; the second composite laminate is close to the buffer layer, and is obtained by mixing aramid fiber and carbon fiber and then laminating them with epoxy resin; the buffer layer adopts a composite structure of epoxy resin and foamed aluminum, and the epoxy resin is located on the upper and lower surfaces of the foamed aluminum.

[0007] Based on the further optimization of the above scheme, the crack arrest layer adopts a surface density of 200±10g / m 2 , aramid plain weave fabric with a thickness of 0.2mm to 0.4mm and a warp / weft breaking strength of not less than 5000N / 50mm.

[0008] Based on the further optimization of the above scheme, the anti-bullet layer adopts a volume density of 2.52±0.03g / m 3 , boron carbide ceramics with a thickness of 9.7mm to 10.3mm; the mechanical properties of boron carbide ceramics in the anti-bullet layer are: Vickers hardness ≥ 35GPa, fracture toughness ≥ 3.5MPa·m 1 / 2 , bending strength ≥ 300MPa, compression strength ≥ 2000MPa.

[0009] Based on further optimization of the above solution, the overall thickness of the support layer is 4.9 mm to 5.5 mm, wherein the thickness ratio between the first composite laminate and the second composite laminate is 2.5 to 3.5:2.

[0010] Based on further optimization of the above scheme, in the first composite laminate, the tow ratio of aramid fiber to carbon fiber in the single layer of hybrid fiber is 6-8:3, and the surface density of the single layer of hybrid fiber is 300g / m 2 ~400g / m 2 ; In the first composite laminate, the angle of the fiber bundles between two adjacent layers of mixed fibers is 30° / 60° (that is, between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 30°, and the angle between the warp and weft of the other layer of fiber bundles is 60°, and the radial and weft aramid fibers and carbon fibers of the single layer are arranged in a ratio of 6 to 8:3), and the content of phenolic resin is 20% to 30%.

[0011] Based on further optimization of the above scheme, in the second composite laminate, the tow ratio of aramid fiber to carbon fiber in the single layer of hybrid fiber is 4:5-7, and the surface density of the single layer of hybrid fiber is 350 g / m 2 ~450g / m 2; In the second composite laminate, the angle of the fiber bundles between two adjacent layers of mixed fibers is 0° / 90° (that is, between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 0°, and the angle between the warp and weft of the other layer of fiber bundles is 90°, and the single-layer radial and weft aramid fibers and carbon fibers are arranged in a ratio of 4:5 to 7), and the content of epoxy resin is 35% to 45%.

[0012] Based on further optimization of the above scheme, the thickness of the buffer layer is 2.2 mm to 2.8 mm, and the volume density of the buffer layer is 1.03 ± 0.05 g / cm 3 ; In the buffer layer, the content of epoxy resin is 30% to 50% and the epoxy resin is evenly distributed on the upper and lower surfaces of the foam aluminum.

[0013] Based on the further optimization of the above scheme, the energy absorbing layer has a thickness of 4.5 mm to 5.5 mm and a volume density of 0.97 ± 0.02 g / cm 3 Ultra-high molecular weight polyethylene laminate.

[0014] A method for preparing a lightweight bullet-resistant and explosion-proof composite armor for a helicopter, comprising: Step 1: Preparation of crack arrest layer: weaving aramid fiber into aramid plain weave cloth with a density of 9 to 11 strands / cm in warp and weft directions to obtain a crack arrest layer for standby use; Step 2: Preparation of support layer: Preparing a first composite laminate: firstly, aramid fiber and carbon fiber are arranged at a tow ratio of 6 to 8:3, and mixed and woven at warp and weft angles of 30° and 60°, respectively, to obtain a plurality of first hybrid fiber plain fabrics, and then the first hybrid fiber plain fabrics are sequentially impregnated in phenolic resin to prepare prepregs, and finally the plurality of prepregs are sequentially stacked at an angle of 30° / 60° (i.e., stacked in a manner of 30°-60°-30°-60°-… until the thickness requirement is met), and compression molded to obtain a first composite laminate; Preparing a second composite laminate: firstly arranging aramid fiber and carbon fiber at a tow ratio of 4:5-7, and respectively mixing and weaving at warp and weft angles of 0° and 90° to obtain a plurality of layers of second hybrid fiber plain fabric, then successively impregnating the second hybrid fiber plain fabric in epoxy resin to prepare a prepreg, and finally successively stacking the plurality of layers of prepreg at an angle of 0° / 90° (i.e., stacking in a manner of 0°-90°-0°-90°-… until the thickness requirement is met), and performing compression molding to obtain a second composite laminate; The first composite laminate is combined with the second composite laminate: the first composite laminate, the epoxy medium temperature curing hot melt adhesive film, and the second composite laminate are stacked and placed in a vacuum bag in sequence, and pre-evacuated to -0.1 MPa, and maintained at room temperature for 15 minutes to 20 minutes; then, the vacuum bag with the composite layer is transferred to an autoclave for hot pressing composite molding to obtain a support layer for standby use; Step 3, buffer layer preparation: first, place a polytetrafluoroethylene isolation film in the groove formed by the silicone rubber, and spread epoxy resin on the surface of the polytetrafluoroethylene isolation film in the groove; then, place the pre-prepared foamed aluminum on the surface of the epoxy resin in the groove, pour epoxy resin on the surface of the foamed aluminum, and lay a layer of polytetrafluoroethylene isolation film on the poured epoxy resin surface; then, place a silicone rubber flat plate on the groove to seal the silicone rubber groove, and place the entire container in a vacuum bag, perform vacuum packaging, and hot press compounding to obtain a buffer layer for use; Step 4: preparing the energy absorbing layer: stacking the ultra-high molecular weight polyethylene non-woven fabric in sequence at an angle of 0° / 90° and compression molding to obtain an energy absorbing layer for standby use; Step 5. Preparation of composite armor: First, the prepared crack-stop layer, bullet-resistant layer, support layer, buffer layer and energy-absorbing layer are cut and processed according to size, and wiped with alcohol; then, the layers are laid in sequence. During the laying process, the connecting surfaces of each layer are bonded with a polyethylene fast-curing hot-melt adhesive film; then, the stacked composite layer is placed in a vacuum bag, and pre-vacuumed to -0.1MPa, and maintained at room temperature for 15min to 20min; then, the vacuum bag with the composite layer is transferred to an autoclave for hot pressing and composite molding to obtain a composite armor.

[0015] Based on further optimization of the above scheme, in the step 2, the molding temperature of the first composite laminate is 170℃~190℃, the pressure is 15MPa~25 MPa, and the insulation and pressure holding time is 90min~120min; the molding temperature of the second composite laminate is 160℃~170℃, the pressure is 15MPa~25 MPa, and the insulation and pressure holding time is 60min~90min; the composite temperature of the first composite laminate and the second composite laminate is 120℃~140℃, the pressure is 2.5MPa~4 MPa, and the insulation and pressure holding time is 60min~100min.

[0016] Based on further optimization of the above scheme, the epoxy resin in step three adopts a high-strength and tough epoxy resin with a viscosity of 6000MPa·s to 10000MPa·s; in step three, the vacuum bag is kept warm at 160°C to 180°C for 90min to 110min.

[0017] Based on further optimization of the above scheme, in step 4, the molding temperature is 120° C. to 130° C., the pressure is 15 MPa to 25 MPa, and the heat preservation and pressure holding time is 90 min to 120 min.

[0018] Based on further optimization of the above scheme, in step five, the curing temperature of the autoclave is 1.8MPa-2.2MPa, the temperature is 110°C-120°C, and the heat preservation and pressure holding time is 70min-80min.

[0019] The present invention has the following technical effects: The composite armor of the present application is a structural combination of a support layer of a first composite laminate and a second composite laminate and a buffer layer of epoxy resin and foamed aluminum, and a multi-resin system of phenolic resin and epoxy resin is used. Firstly, the bonding strength between the layers is improved to avoid obvious stratification problems, thereby ensuring the overall protective performance of the composite armor; secondly, through the system combination of phenolic resin, epoxy resin, carbon fiber and aramid fiber, while ensuring the flame retardancy and ablation resistance of the support layer, it can ensure that the support layer has high bending strength, thereby improving the synergistic matching effect of the support layer and its two adjacent layers (it cooperates with the anti-bullet layer to resist projectiles and block combustion damage, and cooperates with the buffer layer to disperse and consume energy and improve the overall collapse energy absorption effect). ), greatly improving the energy absorption ratio of the anti-ballistic layer, thereby achieving effective protection against high-speed projectile impacts and efficient dissipation of shock wave energy, avoiding problems such as accelerated damage of composite armor under high temperature and high shock waves; in addition, by utilizing the combination of epoxy resin and foamed aluminum, the surface flatness of the aluminum foam is improved through epoxy resin to form a structural layer with a smooth surface and no holes and a porous interior. First, it effectively improves the bonding strength between the buffer layer and the adjacent structural layer, avoiding the active falling off of the structural layer during the impact process and affecting the protective effect. Second, it improves the overall structural strength of the buffer layer and ensures support energy absorption under impact. Third, it uses a porous structure for energy absorption and buffering, and cooperates with the fiber-resin system of the support layer to effectively offset the energy of shock waves during the impact.

[0020] The lightweight bulletproof and explosion-proof composite armor for helicopters in this application can ensure low surface density and an overall surface density of no more than 41.5 kg / m 2 Under the condition of thin thickness and thickness not exceeding 25mm, it can effectively defend against 12.7mm armor-piercing incendiary bullets with a speed of 488m / s and 1.1g simulated fragmentation bullets with a speed of 2000m / s, with good protection effect; at the same time, the composite armor of this application also has excellent sound insulation performance, sound insulation exceeding 35dB and flame retardant performance, which can effectively avoid the problems of accelerated aging and peeling of the structural layer caused by sound waves and high-temperature combustion during the attack. The overall performance is excellent, which can effectively improve the survivability and maneuverability of helicopters during low-altitude combat, and reduce the probability of damage to passengers and key equipment after being attacked. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of the structure of the composite armor in an embodiment of the present invention.

[0022] Among them, 10, crack-stop layer; 20, anti-bullet layer; 30, support layer; 31, first composite laminate; 32, second composite laminate; 40, buffer layer; 50, energy-absorbing layer. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly described below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0024] Embodiment 1: A lightweight bullet-proof and explosion-proof composite armor for a helicopter, comprising a crack-stop layer 10, an anti-bullet layer 20, a support layer 30, a buffer layer 40 and an energy-absorbing layer 50 arranged in sequence; Wherein: the crack arresting layer 10 adopts a surface density of 200±10g / m 2 , aramid plain weave fabric with a thickness of 0.2mm and a warp / weft breaking strength of not less than 5000N / 50mm.

[0025] The anti-ballistic layer 20 has a volume density of 2.52±0.03g / m 3 , boron carbide ceramic with a thickness of 9.7 mm; the mechanical properties of the boron carbide ceramic of the anti-bullet layer 20 are: Vickers hardness ≥ 35 GPa, fracture toughness ≥ 3.5 MPa·m 1 / 2 , bending strength ≥ 300MPa, compression strength ≥ 2000MPa.

[0026] The support layer 30 is a composite laminate of aramid fiber and carbon fiber mixed with a multi-resin system, including a first composite laminate 31 and a second composite laminate 32; the first composite laminate 31 is close to the anti-ballistic layer 20, and is obtained by mixing aramid fiber and carbon fiber and then laminating with phenolic resin; in the first composite laminate 31, the tow ratio of aramid fiber to carbon fiber in a single layer of mixed fiber is 6:3, and the surface density of the single layer of mixed fiber is 300g / m 2; In the first composite laminate 31, the angle of the fiber bundles between two adjacent layers of mixed fibers is 30° / 60° (that is, between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 30°, and the angle between the warp and weft of the other layer of fiber bundles is 60°, and the radial and weft aramid fibers and carbon fibers of a single layer are arranged in a ratio of 6 to 3), and the content of phenolic resin is 20%. The second composite laminate 32 is close to the buffer layer 40, and is obtained by mixing aramid fibers and carbon fibers and then laminating them with epoxy resin; in the second composite laminate 32, the ratio of aramid fibers to carbon fibers in a single layer of mixed fibers is 4:5, and the surface density of the single layer of mixed fibers is 350 g / m 2 ; In the second composite laminate 32, the angle of the fiber bundles between two adjacent layers of mixed fibers is 0° / 90° (i.e., between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 0°, and the angle between the warp and weft of the other layer of fiber bundles is 90°, and the single-layer radial and weft aramid fibers and carbon fibers are arranged in a ratio of 4:5), and the content of epoxy resin is 35%. The overall thickness of the support layer 30 is 4.9 mm, and the thickness ratio between the first composite laminate 31 and the second composite laminate 32 is 2.9:2 (i.e., the thickness of the first composite laminate 31 is 2.9 mm, and the thickness of the second composite laminate 32 is 2 mm).

[0027] The buffer layer 40 is a composite structure of epoxy resin and foamed aluminum, and the epoxy resin is located on the upper and lower surfaces of the foamed aluminum. The buffer layer 40 is 2.2 mm thick and has a volume density of 1.03 ± 0.05 g / cm 3 In the buffer layer 40, the content of epoxy resin is 20% and the epoxy resin is evenly distributed on the upper and lower surfaces of the foamed aluminum.

[0028] The energy absorbing layer 50 has a thickness of 4.5 mm and a volume density of 0.97 ± 0.02 g / cm 3 Ultra-high molecular weight polyethylene laminate.

[0029] The preparation method of the composite armor comprises: Step 1, preparation of the crack-stop layer 10: weave aramid fibers into aramid plain weave cloth with a density of 9 strands / cm in the warp and weft directions to obtain the crack-stop layer 10 for standby use.

[0030] Step 2: Preparation of support layer 30: Preparation of the first composite laminate 31: firstly, aramid fiber and carbon fiber are arranged in a tow ratio of 6:3, and mixedly woven at warp and weft angles of 30° and 60° respectively (i.e., multiple layers are woven at warp and weft angles of 30° for standby use, and multiple layers are woven at warp and weft angles of 60° for standby use), to obtain multiple layers of first mixed fiber plain cloth, and then the first mixed fiber plain cloth is successively impregnated in phenolic resin to form a prepreg, and finally the multiple layers of prepreg are successively stacked at an angle of 30° / 60° (i.e., stacked in a manner of 30°-60°-30°-60°-… until the thickness requirement is met), and molded to obtain the first composite laminate 31; wherein the molding temperature of the first composite laminate 31 is 170°C, the pressure is 15MPa, and the heat preservation and pressure holding time is 90min; Preparation of the second composite laminate 32: firstly, aramid fiber and carbon fiber are arranged in a tow ratio of 4:5, and mixedly woven at warp and weft angles of 0° and 90° respectively (i.e., multiple layers are woven at warp and weft angles of 0° for standby use, and multiple layers are woven at warp and weft angles of 90° for standby use), to obtain multiple layers of second mixed fiber plain weave cloth, and then the second mixed fiber plain weave cloth is successively impregnated in epoxy resin to form prepreg, and finally, multiple layers of prepreg are successively stacked at angles of 0° / 90° (i.e., stacked in a manner of 0°-90°-0°-90°-… until the thickness requirement is met), and molded to obtain the second composite laminate 32; wherein, the molding temperature of the second composite laminate 32 is 160°C, the pressure is 15MPa, and the heat preservation and pressure holding time is 60min; The first composite laminate 31 is combined with the second composite laminate 32: the first composite laminate 31, the epoxy medium-temperature curing hot melt adhesive film and the second composite laminate 32 are stacked and placed in a vacuum bag in sequence, and pre-evacuated to -0.1MPa and maintained at room temperature for 15 minutes; then, the vacuum bag with the composite layer is transferred to an autoclave for hot pressing composite molding to obtain a support layer 30 for standby use; the composite temperature of the first composite laminate 31 and the second composite laminate 32 is 120°C, the pressure is 2.5MPa, and the heat preservation and pressure holding time is 60min.

[0031] Step 3, preparation of buffer layer 40: First, a polytetrafluoroethylene isolation film is placed in the groove formed by the silicone rubber, and epoxy resin is spread on the surface of the polytetrafluoroethylene isolation film in the groove, and the epoxy resin uses a high-strength and tough epoxy resin with a viscosity of 6000 MPa·s; then, the pre-prepared foamed aluminum is placed on the epoxy resin surface in the groove, and then the epoxy resin is poured on the surface of the foamed aluminum, and a layer of polytetrafluoroethylene isolation film is stacked on the poured epoxy resin surface; then, a silicone rubber flat plate is placed on the groove to form a seal for the silicone rubber groove, and the entire container is placed in a vacuum bag, vacuumed and packaged, hot-pressed and compounded at 160°C, and kept warm for 90 minutes to obtain a buffer layer 40 for use.

[0032] Step 4, preparation of energy absorbing layer 50: stack ultra-high molecular weight polyethylene non-woven fabric in sequence at an angle of 0° / 90° and compression mold it to obtain energy absorbing layer 50 for standby use; wherein the compression molding temperature is 120°C, the pressure is 15MPa, and the heat preservation and pressure holding time is 90min.

[0033] Step 5, preparation of composite armor: First, the prepared crack-stop layer 10, bullet-proof layer 20 (the bullet-proof layer 20 can directly use existing boron carbide ceramic raw materials, that is, boron carbide ceramics of a specific thickness are selected as the bullet-proof layer 20), support layer 30, buffer layer 40 and energy-absorbing layer 50 are cut and processed according to size, and wiped with alcohol; then, the layers are laid in sequence. During the laying process, the connecting surfaces of each layer are bonded with a polyethylene-based fast-curing hot-melt adhesive film; then, the stacked composite layer is placed in a vacuum bag, and pre-vacuumed to -0.1MPa, and maintained at room temperature for 15 minutes; then, the vacuum bag with the composite layer is transferred to an autoclave for hot-pressing composite molding. The curing temperature of the autoclave is 1.8MPa, the temperature is 110°C, and the heat preservation and pressure holding time is 70 minutes to obtain a composite armor.

[0034] Embodiment 2: A lightweight bullet-proof and explosion-proof composite armor for a helicopter, comprising a crack-stop layer 10, an anti-bullet layer 20, a support layer 30, a buffer layer 40 and an energy-absorbing layer 50 arranged in sequence; Wherein: the crack arresting layer 10 adopts a surface density of 200±10g / m 2 , aramid plain weave fabric with a thickness of 0.3mm and a warp / weft breaking strength of not less than 5000N / 50mm.

[0035] The anti-ballistic layer 20 has a volume density of 2.52±0.03g / m 3 , boron carbide ceramics with a thickness of 10 mm; the mechanical properties of the boron carbide ceramics of the anti-bullet layer 20 are: Vickers hardness ≥ 35 GPa, fracture toughness ≥ 3.5 MPa·m 1 / 2 , bending strength ≥ 300MPa, compression strength ≥ 2000MPa.

[0036] The support layer 30 is a composite laminate of aramid fiber and carbon fiber mixed with a multi-resin system, including a first composite laminate 31 and a second composite laminate 32; the first composite laminate 31 is close to the anti-ballistic layer 20, and is obtained by mixing aramid fiber and carbon fiber and then laminating them with phenolic resin; in the first composite laminate 31, the tow ratio of aramid fiber to carbon fiber in a single layer of mixed fiber is 7:3, and the surface density of the single layer of mixed fiber is 350g / m 2 ; In the first composite laminate 31, the angle of the fiber bundles between two adjacent layers of mixed fibers is 30° / 60° (that is, between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 30°, and the angle between the warp and weft of the other layer of fiber bundles is 60°, and the radial and weft aramid fibers and carbon fibers of a single layer are arranged in a ratio of 7:3), and the content of phenolic resin is 25%. The second composite laminate 32 is close to the buffer layer 40, and is obtained by mixing aramid fibers and carbon fibers and then laminating them with epoxy resin; in the second composite laminate 32, the ratio of aramid fibers to carbon fibers in a single layer of mixed fibers is 4:6, and the surface density of the single layer of mixed fibers is 400g / m 2 ; In the second composite laminate 32, the angle of the fiber bundles between two adjacent layers of mixed fibers is 0° / 90° (i.e., between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 0°, and the angle between the warp and weft of the other layer of fiber bundles is 90°, and the single-layer radial and weft aramid fibers and carbon fibers are arranged in a ratio of 4:6), and the content of epoxy resin is 40%. The overall thickness of the support layer 30 is 5mm, and the thickness ratio between the first composite laminate 31 and the second composite laminate 32 is 3:2 (i.e., the thickness of the first composite laminate 31 is 3mm, and the thickness of the second composite laminate 32 is 2mm).

[0037] The buffer layer 40 is a composite structure of epoxy resin and foamed aluminum, and the epoxy resin is located on the upper and lower surfaces of the foamed aluminum. The buffer layer 40 is 2.5 mm thick and has a volume density of 1.03 ± 0.05 g / cm 3 In the buffer layer 40, the content of epoxy resin is 30% and the epoxy resin is evenly distributed on the upper and lower surfaces of the foamed aluminum.

[0038] The energy absorbing layer 50 has a thickness of 5 mm and a volume density of 0.97 ± 0.02 g / cm 3 Ultra-high molecular weight polyethylene laminate.

[0039] The preparation method of the composite armor comprises: Step 1, preparation of the crack-stop layer 10: weave aramid fibers into aramid plain weave cloth with a density of 10 strands / cm in the warp and weft directions to obtain the crack-stop layer 10 for standby use.

[0040] Step 2: Preparation of support layer 30: Preparation of the first composite laminate 31: firstly, aramid fiber and carbon fiber are arranged in a tow ratio of 7:3, and mixedly woven at warp and weft angles of 30° and 60° respectively (i.e., multiple layers are woven at warp and weft angles of 30° for standby use, and multiple layers are woven at warp and weft angles of 60° for standby use), to obtain multiple layers of first mixed fiber plain cloth, and then the first mixed fiber plain cloth is successively impregnated in phenolic resin to form a prepreg, and finally the multiple layers of prepreg are successively stacked at an angle of 30° / 60° (i.e., stacked in a manner of 30°-60°-30°-60°-… until the thickness requirement is met), and molded to obtain the first composite laminate 31; wherein the molding temperature of the first composite laminate 31 is 180°C, the pressure is 20MPa, and the heat preservation and pressure holding time is 115min; Preparation of the second composite laminate 32: firstly, aramid fiber and carbon fiber are arranged in a tow ratio of 4:6, and mixedly woven at warp and weft angles of 0° and 90° respectively (i.e., multiple layers are woven at warp and weft angles of 0° for standby use, and multiple layers are woven at warp and weft angles of 90° for standby use), to obtain multiple layers of second mixed fiber plain weave cloth, and then the second mixed fiber plain weave cloth is successively impregnated in epoxy resin to form prepreg, and finally, multiple layers of prepreg are successively stacked at angles of 0° / 90° (i.e., stacked in a manner of 0°-90°-0°-90°-… until the thickness requirement is met), and molded to obtain the second composite laminate 32; wherein, the molding temperature of the second composite laminate 32 is 165°C, the pressure is 20 MPa, and the heat preservation and pressure holding time is 75min; The first composite laminate 31 is combined with the second composite laminate 32: the first composite laminate 31, the epoxy medium-temperature curing hot melt adhesive film and the second composite laminate 32 are stacked and placed in a vacuum bag in sequence, and pre-evacuated to -0.1MPa and maintained at room temperature for 17 minutes; then, the vacuum bag with the composite layer is transferred to an autoclave for hot pressing composite molding to obtain a support layer 30 for standby use; the composite temperature of the first composite laminate 31 and the second composite laminate 32 is 130°C, the pressure is 3MPa, and the heat preservation and pressure holding time is 80min.

[0041] Step 3, preparation of buffer layer 40: First, a polytetrafluoroethylene isolation film is placed in the groove formed by the silicone rubber, and epoxy resin is spread on the surface of the polytetrafluoroethylene isolation film in the groove, and the epoxy resin uses a high-strength and tough epoxy resin with a viscosity of 8000 MPa·s; then, the pre-prepared foamed aluminum is placed on the surface of the epoxy resin in the groove, and then the epoxy resin is poured on the surface of the foamed aluminum, and a layer of polytetrafluoroethylene isolation film is stacked on the surface of the poured epoxy resin; then, a silicone rubber flat plate is placed on the groove to form a seal for the silicone rubber groove, and the entire container is placed in a vacuum bag, vacuumed and packaged, hot-pressed and compounded at 170°C, and kept warm for 100 minutes to obtain a buffer layer 40 for use.

[0042] Step 4, preparation of energy absorbing layer 50: stack ultra-high molecular weight polyethylene non-woven fabric in sequence at an angle of 0° / 90° and compression mold it to obtain energy absorbing layer 50 for standby use; wherein the compression molding temperature is 125°C, the pressure is 20MPa, and the heat preservation and pressure holding time is 115min.

[0043] Step 5, preparation of composite armor: First, the prepared crack-stop layer 10, bullet-proof layer 20 (the bullet-proof layer 20 can directly use existing boron carbide ceramic raw materials, that is, boron carbide ceramics of a specific thickness are selected as the bullet-proof layer 20), support layer 30, buffer layer 40 and energy-absorbing layer 50 are cut and processed according to size, and wiped with alcohol; then, the layers are laid in sequence. During the laying process, the connecting surfaces of each layer are bonded with a polyethylene-type fast-curing hot-melt adhesive film; then, the stacked composite layer is placed in a vacuum bag, and pre-vacuumed to -0.1MPa, and maintained at room temperature for 17 minutes; then, the vacuum bag with the composite layer is transferred to an autoclave for hot-pressing composite molding. The curing temperature of the autoclave is 2MPa, the temperature is 115°C, and the heat preservation and pressure holding time is 75 minutes to obtain a composite armor.

[0044] Embodiment 3: A lightweight bullet-proof and explosion-proof composite armor for a helicopter, comprising a crack-stop layer 10, an anti-bullet layer 20, a support layer 30, a buffer layer 40 and an energy-absorbing layer 50 arranged in sequence; Wherein: the crack arresting layer 10 adopts a surface density of 200±10g / m 2 , aramid plain weave fabric with a thickness of 0.4mm and a warp / weft breaking strength of not less than 5000N / 50mm.

[0045] The anti-ballistic layer 20 has a volume density of 2.52±0.03g / m 3 , boron carbide ceramic with a thickness of 10.3 mm; the mechanical properties of the boron carbide ceramic of the anti-bullet layer 20 are: Vickers hardness ≥ 35 GPa, fracture toughness ≥ 3.5 MPa·m 1 / 2 , bending strength ≥ 300MPa, compression strength ≥ 2000MPa.

[0046] The support layer 30 is a composite laminate of aramid fiber and carbon fiber mixed with a multi-resin system, including a first composite laminate 31 and a second composite laminate 32; the first composite laminate 31 is close to the anti-ballistic layer 20, and is obtained by mixing aramid fiber and carbon fiber and then laminating with phenolic resin; in the first composite laminate 31, the tow ratio of aramid fiber to carbon fiber in a single layer of mixed fiber is 8:3, and the surface density of the single layer of mixed fiber is 400g / m 2 ; In the first composite laminate 31, the angle of the fiber bundles between two adjacent layers of mixed fibers is 30° / 60° (that is, between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 30°, and the angle between the warp and weft of the other layer of fiber bundles is 60°, and the radial and weft aramid fibers and carbon fibers of the single layer are arranged in a ratio of 8:3), and the content of phenolic resin is 30%. The second composite laminate 32 is close to the buffer layer 40, and is obtained by mixing aramid fibers and carbon fibers and then laminating them with epoxy resin; in the second composite laminate 32, the ratio of aramid fibers to carbon fibers in the single layer of mixed fibers is 4:7, and the surface density of the single layer of mixed fibers is 450g / m 2 ; In the second composite laminate 32, the angle of the fiber bundles between two adjacent layers of mixed fibers is 0° / 90° (i.e., between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 0°, and the angle between the warp and weft of the other layer of fiber bundles is 90°, and the single-layer radial and weft aramid fibers and carbon fibers are arranged in a ratio of 4:7), and the content of epoxy resin is 45%. The overall thickness of the support layer 30 is 5.5mm, and the thickness ratio between the first composite laminate 31 and the second composite laminate 32 is 3.5:2 (i.e., the thickness of the first composite laminate 31 is 3.5mm, and the thickness of the second composite laminate 32 is 2mm).

[0047] The buffer layer 40 is a composite structure of epoxy resin and foamed aluminum, and the epoxy resin is located on the upper and lower surfaces of the foamed aluminum. The buffer layer 40 is 2.8 mm thick and has a volume density of 1.03 ± 0.05 g / cm 3 In the buffer layer 40, the content of epoxy resin is 40% and the epoxy resin is evenly distributed on the upper and lower surfaces of the foamed aluminum.

[0048] The energy absorbing layer 50 has a thickness of 5.5 mm and a volume density of 0.97 ± 0.02 g / cm 3 Ultra-high molecular weight polyethylene laminate.

[0049] The preparation method of the composite armor comprises: Step 1, preparation of the crack-stop layer 10: weave aramid fibers into aramid plain weave cloth with a density of 11 strands / cm in the warp and weft directions to obtain the crack-stop layer 10 for standby use.

[0050] Step 2: Preparation of support layer 30: Preparation of the first composite laminate 31: firstly, aramid fiber and carbon fiber are arranged in a tow ratio of 8:3, and mixedly woven at warp and weft angles of 30° and 60° respectively (i.e., multiple layers are woven at warp and weft angles of 30° for standby use, and multiple layers are woven at warp and weft angles of 60° for standby use), to obtain multiple layers of first mixed fiber plain cloth, and then the first mixed fiber plain cloth is successively impregnated in phenolic resin to form a prepreg, and finally the multiple layers of prepreg are successively stacked at an angle of 30° / 60° (i.e., stacked in a manner of 30°-60°-30°-60°-… until the thickness requirement is met), and molded to obtain the first composite laminate 31; wherein the molding temperature of the first composite laminate 31 is 190°C, the pressure is 25 MPa, and the heat preservation and pressure holding time is 120min; Preparation of the second composite laminate 32: firstly, aramid fiber and carbon fiber are arranged in a tow ratio of 4:7, and mixedly woven at warp and weft angles of 0° and 90° respectively (i.e., multiple layers are woven at warp and weft angles of 0° for standby use, and multiple layers are woven at warp and weft angles of 90° for standby use), to obtain multiple layers of second mixed fiber plain weave cloth, and then the second mixed fiber plain weave cloth is successively impregnated in epoxy resin to form prepreg, and finally, multiple layers of prepreg are successively stacked at angles of 0° / 90° (i.e., stacked in a manner of 0°-90°-0°-90°-… until the thickness requirement is met), and molded to obtain the second composite laminate 32; wherein, the molding temperature of the second composite laminate 32 is 170°C, the pressure is 25 MPa, and the heat preservation and pressure holding time is 90 min; The first composite laminate 31 is combined with the second composite laminate 32: the first composite laminate 31, the epoxy medium-temperature curing hot melt adhesive film, and the second composite laminate 32 are stacked and placed in a vacuum bag in sequence, and pre-evacuated to -0.1 MPa and maintained at room temperature for 20 minutes; then, the vacuum bag with the composite layer is transferred to an autoclave for hot pressing composite molding to obtain a support layer 30 for standby use; the composite temperature of the first composite laminate 31 and the second composite laminate 32 is 140°C, the pressure is 4 MPa, and the heat preservation and pressure holding time is 100 minutes.

[0051] Step 3, preparation of buffer layer 40: First, place a polytetrafluoroethylene isolation film in the groove formed by the silicone rubber, and spread epoxy resin on the surface of the polytetrafluoroethylene isolation film in the groove, and the epoxy resin uses a high-strength and tough epoxy resin with a viscosity of 10000 MPa·s; then, place the pre-prepared foamed aluminum on the surface of the epoxy resin in the groove, pour epoxy resin on the surface of the foamed aluminum, and lay a layer of polytetrafluoroethylene isolation film on the poured epoxy resin surface; then, place a silicone rubber flat plate on the groove to seal the silicone rubber groove, and place the entire container in a vacuum bag, vacuum package it, perform hot pressing and compounding at 180°C, and keep it warm for 110 minutes to obtain the buffer layer 40 for use.

[0052] Step 4, preparation of energy absorbing layer 50: stack ultra-high molecular weight polyethylene non-woven fabric in sequence at an angle of 0° / 90° and compression mold it to obtain energy absorbing layer 50 for standby use; wherein the compression molding temperature is 130°C, the pressure is 25MPa, and the heat preservation and pressure holding time is 120min.

[0053] Step 5, preparation of composite armor: First, the prepared crack-stop layer 10, bullet-proof layer 20 (the bullet-proof layer 20 can directly use existing boron carbide ceramic raw materials, that is, boron carbide ceramics of a specific thickness are selected as the bullet-proof layer 20), support layer 30, buffer layer 40 and energy-absorbing layer 50 are cut and processed according to size, and wiped with alcohol; then, the layers are laid in sequence, and during the laying process, the connecting surfaces of each layer are bonded with a polyethylene-type fast-curing hot-melt adhesive film; then, the stacked composite layer is placed in a vacuum bag, and pre-vacuumed to -0.1MPa, and maintained at room temperature for 20 minutes; then, the vacuum bag with the composite layer is transferred to an autoclave for hot-pressing composite molding. The curing temperature of the autoclave is 2.2MPa, the temperature is 120°C, and the heat preservation and pressure holding time is 80 minutes to obtain a composite armor.

[0054] Comparative Example 1: A composite layer for a helicopter, comprising a crack arresting layer, an anti-ballistic layer, a supporting layer, a buffer layer and an energy absorbing layer arranged in sequence; Wherein: the crack-stopping layer is consistent with the crack-stopping layer in Example 2.

[0055] The anti-ballistic layer is consistent with the anti-ballistic layer in Example 2.

[0056] The support layer 30 is a composite laminate of aramid fiber and carbon fiber mixed with a multi-resin system, including a first composite laminate 31 and a second composite laminate 32; the first composite laminate 31 is close to the anti-ballistic layer 20, and is obtained by mixing aramid fiber and carbon fiber and then laminating them with epoxy resin; in the first composite laminate 31, the tow ratio of aramid fiber to carbon fiber in a single layer of mixed fiber is 7:3, and the surface density of the single layer of mixed fiber is 350g / m 2; In the first composite laminate 31, the angle of the fiber bundles between two adjacent layers of mixed fibers is 30° / 60° (that is, between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 30°, and the angle between the warp and weft of the other layer of fiber bundles is 60°, and the radial and weft aramid fibers and carbon fibers of a single layer are arranged in a ratio of 7:3), and the content of epoxy resin is 40%. The second composite laminate 32 is close to the buffer layer 40, and is obtained by mixing aramid fibers and carbon fibers and then laminating them with phenolic resin; in the second composite laminate 32, the ratio of aramid fibers to carbon fibers in a single layer of mixed fibers is 4:6, and the surface density of the single layer of mixed fibers is 400g / m 2 ; In the second composite laminate 32, the angle of the fiber bundles between two adjacent layers of mixed fibers is 0° / 90° (i.e., between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 0°, and the angle between the warp and weft of the other layer of fiber bundles is 90°, and the single-layer radial and weft aramid fibers and carbon fibers are arranged in a ratio of 4:6), and the content of phenolic resin is 25%. The overall thickness of the support layer 30 is 5mm, and the thickness ratio between the first composite laminate 31 and the second composite laminate 32 is 3:2 (i.e., the thickness of the first composite laminate 31 is 3mm, and the thickness of the second composite laminate 32 is 2mm).

[0057] The buffer layer is consistent with the buffer layer in Example 2.

[0058] The energy absorbing layer is consistent with the energy absorbing layer in Example 2.

[0059] The composite layer is prepared by a method similar to that in Example 2.

[0060] Comparative Example 2: A composite layer for a helicopter, comprising a crack arresting layer, an anti-ballistic layer, a supporting layer, a buffer layer and an energy absorbing layer arranged in sequence; Wherein: the crack-stopping layer is consistent with the crack-stopping layer in Example 2.

[0061] The anti-ballistic layer is consistent with the anti-ballistic layer in Example 2.

[0062] The support layer is made of aramid fiber and carbon fiber mixed composite laminate under epoxy resin system, among which the tow ratio of aramid fiber to carbon fiber in a single layer of mixed fiber is 7:3, and the surface density of the single layer of mixed fiber is 350g / m 2 The angle of the fiber bundles between two adjacent layers of mixed fibers is 30° / 60° (that is, between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 30°, and the angle between the warp and weft of the other layer of fiber bundles is 60°, and the single-layer radial or weft aramid fiber and carbon fiber are arranged in a ratio of 7:3), and the content of epoxy resin is 40%; the overall thickness of the support layer is 5mm.

[0063] The buffer layer is consistent with the buffer layer in Example 2.

[0064] The energy absorbing layer is consistent with the energy absorbing layer in Example 2.

[0065] The composite layer is prepared by a method similar to that in Example 2.

[0066] Comparative Example 3: A composite layer for a helicopter, comprising a crack arresting layer, an anti-ballistic layer, a supporting layer, a buffer layer and an energy absorbing layer arranged in sequence; Wherein: the crack-stopping layer is consistent with the crack-stopping layer in Example 2.

[0067] The anti-ballistic layer is consistent with the anti-ballistic layer in Example 2.

[0068] The support layer is a composite laminate of aramid fiber and carbon fiber mixed under a phenolic resin system, wherein the tow ratio of aramid fiber to carbon fiber in a single layer of mixed fiber is 4:6, and the surface density of the single layer of mixed fiber is 400g / m 2 The angle of the fiber bundles between two adjacent layers of mixed fibers is 0° / 90° (that is, between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 0°, and the angle between the warp and weft of the other layer of fiber bundles is 90°, and the radial and weft aramid fibers and carbon fibers of a single layer are arranged in a ratio of 4:6), and the content of phenolic resin is 25%; the overall thickness of the support layer is 5mm.

[0069] The buffer layer is consistent with the buffer layer in Example 2.

[0070] The energy absorbing layer is consistent with the energy absorbing layer in Example 2.

[0071] The composite layer is prepared by a method similar to that in Example 2.

[0072] Comparative Example 4: A composite layer for a helicopter, comprising a crack arresting layer, an anti-ballistic layer, a supporting layer, a buffer layer and an energy absorbing layer arranged in sequence; Wherein: the crack-stopping layer is consistent with the crack-stopping layer in Example 2.

[0073] The anti-ballistic layer is consistent with the anti-ballistic layer in Example 2.

[0074] The supporting layer adopts a composite laminate of aramid fiber and carbon fiber mixed with a multi-resin system, including a first composite laminate and a second composite laminate; the first composite laminate is close to the anti-ballistic layer, and is obtained by mixing aramid fiber and carbon fiber and then laminating them with phenolic resin; in the first composite laminate, the tow ratio of aramid fiber to carbon fiber in a single layer of mixed fiber is 4:6, and the surface density of the single layer of mixed fiber is 400g / m 2; In the first composite laminate, the angle of the fiber bundles between two adjacent layers of mixed fibers is 0° / 90° (that is, between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 0°, and the angle between the warp and weft of the other layer of fiber bundles is 90°, and the radial and weft aramid fibers and carbon fibers of a single layer are arranged in a ratio of 4:6), and the content of phenolic resin is 25%. The second composite laminate is close to the buffer layer and is obtained by mixing aramid fibers and carbon fibers and then laminating them with epoxy resin; in the second composite laminate, the ratio of aramid fibers to carbon fibers in a single layer of mixed fibers is 7:3, and the surface density of a single layer of mixed fibers is 350g / m 2 ; In the second composite laminate, the angle of the fiber bundles between two adjacent layers of mixed fibers is 30° / 60° (i.e., between two adjacent layers of mixed fibers, the angle between the warp and weft of one layer of fiber bundles is 30°, and the angle between the warp and weft of the other layer of fiber bundles is 60°, and the single-layer radial or weft aramid fiber and carbon fiber are arranged in a ratio of 7:3), and the content of epoxy resin is 40%. The overall thickness of the support layer is 5mm, and the thickness ratio between the first composite laminate and the second composite laminate is 3:2 (i.e., the thickness of the first composite laminate is 3mm, and the thickness of the second composite laminate is 2mm).

[0075] The buffer layer is consistent with the buffer layer in Example 2.

[0076] The energy absorbing layer is consistent with the energy absorbing layer in Example 2.

[0077] The composite layer is prepared by a method similar to that in Example 2.

[0078] Comparative Example 5: A composite layer for a helicopter, comprising a crack arresting layer, an anti-ballistic layer, a supporting layer, a buffer layer and an energy absorbing layer arranged in sequence; Wherein: the crack-stopping layer is consistent with the crack-stopping layer in Example 2.

[0079] The anti-ballistic layer is consistent with the anti-ballistic layer in Example 2.

[0080] The support layer is consistent with the support layer in Example 2.

[0081] The buffer layer adopts a composite structure of epoxy resin and honeycomb aluminum; the thickness of the buffer layer is 2.5mm, and the volume density of the buffer layer is 1.03±0.05g / cm 3 ; In the buffer layer, the content of epoxy resin is 30% and the epoxy resin is evenly coated on the upper and lower surfaces of the honeycomb aluminum.

[0082] The energy absorbing layer is consistent with the energy absorbing layer in Example 2.

[0083] The composite layer is prepared by a method similar to that in Example 2.

[0084] The bullet-proof and explosion-proof composite armors in Examples 1 to 3 and the composite layers in Comparative Examples 1 to 5 were respectively subjected to a 12.7 mm incendiary bullet penetration test and a speed greater than or equal to 488 m / s and a sound insulation test. The test results are shown in the following table:

[0085] It can be clearly seen from the above table that when the tow ratio, single layer stacking angle and resin system in the support layer change, the protective ability of the composite layer will be significantly affected. From the results of Example 2 and Comparative Example 1, it can be seen that when the resin system changes, the sound insulation will not decrease significantly and the composite layer is not penetrated, but the deformation of the back of the composite layer increases significantly; from the results of Example 2, Comparative Example 2 and Comparative Example 3, it can be seen that when the support layer adopts a single resin system, although the sound insulation will not decrease significantly, the composite layer is directly penetrated, indicating that the protective effect of the single resin system is extremely poor; from the results of Example 2 and Comparative Example 4, it can be seen that when the tow ratio and stacking angle between aramid fiber and carbon fiber change, even if the same resin system is used, the deformation of the back of the composite layer will increase significantly. In addition, from Example 2 and Comparative Example 5, it can be seen that the combination of epoxy resin and foam aluminum in the buffer layer has obvious advantages in terms of protective effect and sound insulation compared with the combination of epoxy resin and honeycomb aluminum.

Claims

1. A lightweight bulletproof and explosion-proof composite armor for helicopters, characterized by: It includes a crack-arresting layer, an anti-ballistic layer, a supporting layer, a buffer layer and an energy-absorbing layer which are arranged in sequence; the supporting layer adopts a composite laminate of aramid fiber and carbon fiber mixed with a multi-resin system, including a first composite laminate and a second composite laminate; the first composite laminate is close to the anti-ballistic layer, and is obtained by mixing aramid fiber and carbon fiber and then laminating them with phenolic resin; the second composite laminate is close to the buffer layer, and is obtained by mixing aramid fiber and carbon fiber and then laminating them with epoxy resin; the buffer layer adopts a composite structure of epoxy resin and foamed aluminum, and the epoxy resin is located on the upper and lower surfaces of the foamed aluminum.

2. The lightweight bulletproof and explosion-proof composite armor for helicopters according to claim 1, characterized in that: The crack arresting layer has a surface density of 200±10g / m 2 , aramid plain weave fabric with a thickness of 0.2mm to 0.4mm and a warp / weft breaking strength of not less than 5000N / 50mm.

3. A lightweight bullet-proof and explosion-proof composite armor for helicopters according to claim 1 or 2, characterized in that: The anti-ballistic layer has a volume density of 2.52±0.03 g / m 3 , boron carbide ceramics with a thickness of 9.7mm to 10.3mm; the mechanical properties of boron carbide ceramics in the anti-bullet layer are: Vickers hardness ≥ 35GPa, fracture toughness ≥ 3.5MPa·m 1 / 2 , bending strength ≥ 300MPa, compression strength ≥ 2000MPa.

4. A lightweight bulletproof and explosion-proof composite armor for helicopters according to any one of claims 1 to 3, characterized in that: The overall thickness of the support layer is 4.9 mm to 5.5 mm, wherein the thickness ratio between the first composite laminate and the second composite laminate is 2.5 to 3.5:

2.

5. A lightweight bullet-proof and explosion-proof composite armor for helicopters according to any one of claims 1 to 4, characterized in that: In the first composite laminate, the tow ratio of the aramid fiber to the carbon fiber in the single layer of hybrid fiber is 6 to 8:3, and the surface density of the single layer of hybrid fiber is 300 g / m 2 ~400g / m 2 In the first composite laminate, the angle of the fiber bundles between two adjacent layers of mixed fibers is 30° / 60°, and the content of the phenolic resin is 20% to 30%.

6. A lightweight bullet-proof and explosion-proof composite armor for helicopters according to any one of claims 1 to 4, characterized in that: In the second composite laminate, the tow ratio of the aramid fiber to the carbon fiber in the single layer of hybrid fiber is 4:5-7, and the surface density of the single layer of hybrid fiber is 350 g / m 2 ~450g / m 2 ; In the second composite laminate, the angle of the fiber bundles between two adjacent layers of mixed fibers is 0° / 90°, and the content of the epoxy resin is 35% to 45%.

7. The lightweight bulletproof and explosion-proof composite armor for helicopters according to claim 6, characterized in that: The thickness of the buffer layer is 2.2 mm to 2.8 mm, and the volume density of the buffer layer is 1.03 ± 0.05 g / cm 3 ; In the buffer layer, the content of epoxy resin is 30% to 50% and the epoxy resin is evenly distributed on the upper and lower surfaces of the foam aluminum.

8. The lightweight bulletproof and explosion-proof composite armor for helicopters according to claim 6, characterized in that: The energy absorbing layer has a thickness of 4.5 mm to 5.5 mm and a volume density of 0.97 ± 0.02 g / cm 3 Ultra-high molecular weight polyethylene laminate.

Citation Information

Cited By

  • Novel hybrid fiber composite material as well as preparation method and application thereof

    CN119550703A

  • Hybrid fiber composite, method for producing same, and use thereof

    CN119550703B

  • Lightweight hybrid fiber bulletproof flashboard and preparation method thereof

    CN120941838A

  • Lightweight hybrid fiber bulletproof plugboard and preparation method

    CN120941838B