Sodium ferric sulfate positive electrode material and preparation method and application thereof

In the preparation of sodium iron sulfate cathode materials, sodium sources, iron sources, etc. are mixed to prepare suspensions and spray-dried and sintered to form a uniform carbon coating layer, which solves the problems caused by uneven coating of polyanionic sodium iron sulfate cathode materials. The problems of poor conductivity and easy failure have significantly improved its electrochemical performance and stability.

CN118724072APending Publication Date: 2024-10-01GEM WUXI ENERGY MATERIAL CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411167744.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Polyanionic sodium ferric sulfate cathode materials are prone to uneven coating, resulting in poor electrical conductivity, easy oxidation by air and water absorption, resulting in difficulty in energy storage performance and easy material failure.

Method used

A sodium source, an iron source, a sulfur source, an antioxidant, an organic carbon source, an inorganic carbon source, a dispersant, and a defoaming agent are mixed to prepare a suspension. The sodium iron sulfate cathode material is prepared through spray drying and sintering to form a uniform carbon package. The coating isolates moisture and carbon dioxide in the air and improves the air stability and electrochemical performance of the material.

Benefits of technology

Uniform carbon coating of the sodium iron sulfate cathode material is achieved, improving its air stability and electrochemical performance, enhancing conductivity, reducing battery polarization, and extending the material's storage capacity and charge transfer efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of sodium ion batteries, and particularly relates to a sodium ferric sulfate positive electrode material as well as a preparation method and application thereof. The preparation method of the sodium ferric sulfate positive electrode material comprises the following steps: S1, mixing a sodium source, an iron source, a sulfur source, an antioxidant, an organic carbon source, an inorganic carbon source, a dispersing agent, a defoaming agent and deionized water to obtain a suspension; s2, carrying out spray drying treatment on the turbid liquid obtained in the step S1 to obtain a sodium ferric sulfate positive electrode material precursor; and S3, sintering the sodium ferric sulfate positive electrode material precursor obtained in the S2 to obtain the sodium ferric sulfate positive electrode material. The surface of the sodium ferric sulfate positive electrode material is provided with a uniform carbon coating layer which can be used as a protective barrier layer to effectively isolate moisture and carbon dioxide in air, so that defect sites are avoided, and the air stability of the sodium ferric sulfate positive electrode material can be improved; and the capability of being stored in a long-term natural environment and excellent electrochemical performance are provided for the sodium ferric sulfate positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a sodium iron sulfate positive electrode material and a preparation method and application thereof. Background Art

[0002] As environmental problems become increasingly severe, the demand for the development of new renewable energy sources is also increasing. Lithium-ion batteries are considered to be a sustainable energy source with good development prospects. With its advantages of high safety, high energy density, and long service life, they have been widely used in various portable mobile devices, electric vehicles, and energy storage. However, due to the extremely uneven distribution of lithium resources in the world and the rapid and large-scale consumption today, its production and use costs will inevitably be affected. Therefore, sodium-ion batteries, which have similar working principles to lithium-ion batteries, have received extensive research and attention in the global energy storage field due to their wide distribution of sodium resources. Among them, the positive electrode material is a key link in the entire battery system, and its cycle stability, output voltage, thermal stability, output capacity, power density and other indicators play a decisive role in the entire battery system. At present, the positive electrode materials of sodium-ion batteries mainly include layered oxides, polyanions, and Prussian blue. Among them, polyanion compounds have significant advantages in sodium-ion battery positive electrode materials due to their open skeleton structure, low-energy ion migration pathways, and adjustable voltage range. In particular, polyanionic sodium iron sulfate positive electrode materials have attracted widespread attention because of their low production cost and high working voltage. However, the conductivity of polyanionic sodium iron sulfate positive electrode materials is generally poor, and the good energy storage properties are difficult to exert. In addition, the material is very easy to absorb water and is easily oxidized by oxygen in the air, which makes the material easy to fail. In the prior art, the method of carbon coating the positive electrode material is often used to overcome the problem of easy failure, but this is prone to uneven coating. The unevenly coated positive electrode material is prone to defective sites that are easily oxidized by air and absorb water, and it also causes some materials to have poor conductivity, and the energy storage performance is difficult to exert, and the material is still prone to failure. Summary of the invention

[0003] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the polyanionic sodium iron sulfate positive electrode materials in the prior art, which are prone to defect sites that are easily oxidized by air and absorb water due to uneven coating during coating, resulting in poor conductivity, difficulty in exerting energy storage performance, and easy material failure, thereby providing a sodium iron sulfate positive electrode material and its preparation method and application.

[0004] To this end, the present invention provides the following technical solutions.

[0005] The invention provides a method for preparing a sodium ferric sulfate positive electrode material, comprising the following steps: S1: mixing a sodium source, an iron source, a sulfur source, an antioxidant, an organic carbon source, an inorganic carbon source, a dispersant, a defoaming agent and deionized water to obtain a suspension; S2: spray drying the suspension obtained in S1 to obtain a sodium ferric sulfate positive electrode material precursor; S3: sintering the sodium ferric sulfate positive electrode material precursor obtained in S2 to obtain the sodium ferric sulfate positive electrode material.

[0006] Optionally, the mass of the organic carbon source is 0.01% to 10% of the sum of the masses of the sodium source, the iron source and the sulfur source.

[0007] Optionally, the mass of the inorganic carbon source is 0.05% to 6% of the sum of the masses of the sodium source, the iron source and the sulfur source.

[0008] Optionally, the mass of the antioxidant is 0.05% to 5% of the sum of the mass of the sodium source, the iron source and the sulfur source.

[0009] Optionally, the mass of the dispersant is 0.1% to 5% of the sum of the masses of the sodium source, the iron source and the sulfur source.

[0010] Optionally, the mass of the defoaming agent is 1-100 ppm of the sum of the masses of the sodium source, the iron source and the sulfur source.

[0011] Optionally, the amount of sodium source, iron source and sulfur source is calculated according to the stoichiometric ratio of sodium ferric sulfate; Optionally, the sodium ferric sulfate is a non-stoichiometric sodium ferric sulfate; Optionally, the chemical formula of the non-stoichiometric sodium ferric sulfate is Na x Fe y (SO4) z , where 2≤x≤3, 1.5≤y≤2, 1≤x / y≤2, x+2y=2z.

[0012] Optionally, the mass of the deionized water is 15% to 40% of the sum of the mass of the sodium source, the iron source, the sulfur source, the antioxidant, the organic carbon source, the inorganic carbon source, the dispersant, and the defoaming agent.

[0013] Optionally, in step S2, the inlet air temperature of the spray drying is 140-280°C, and the outlet air temperature is 70-140°C.

[0014] Optionally, in step S3, the sintering includes a first stage sintering and a second stage sintering, the first stage sintering is performed at a temperature of 100-280°C and a time of 0.1-12 hours, and the second stage sintering is performed at a temperature of 300-400°C and a time of 0.1-24 hours.

[0015] Optionally, in step S1, a stirring step is further included after mixing, and the stirring speed is 100-400 r / min and the stirring time is 2-3 h.

[0016] Optionally, in step S3, sintering is performed under a nitrogen and / or inert gas atmosphere.

[0017] Optionally, in step S3, after sintering, the step of crushing the sintered material is also included.

[0018] Optionally, the organic carbon source is a water-soluble organic carbon source; optionally, the organic carbon source includes at least one of glucose, sucrose, fructose, and water-soluble starch.

[0019] Optionally, the inorganic carbon source includes at least one of acetylene black, graphene, carbon nanotubes, carbon fibers, activated carbon, and conductive carbon black.

[0020] Optionally, the dispersant includes at least one of sodium dodecyl sulfate, polyethylene glycol, sodium alkylbenzene sulfonate, sodium alkyl sulfonate, sodium stearate, and polyvinyl pyrrolidone.

[0021] Optionally, the defoaming agent includes at least one of hydroxymethyl cellulose, polysiloxane, and polyether-modified silicone oil.

[0022] Optionally, the antioxidant is a water-soluble antioxidant; optionally, the antioxidant includes at least one of ascorbic acid, citric acid, phytic acid, uric acid, oxalic acid, formic acid, and acetic acid. Using a water-soluble organic carbon source and a water-soluble antioxidant can avoid Fe 3+ The formation of impurities further improves the electrochemical performance of the positive electrode material.

[0023] Optionally, the sodium source is a soluble salt containing sodium; optionally, the sodium source includes at least one of sodium sulfate, sodium bisulfate, sodium carbonate, sodium bicarbonate, sodium nitrate and sodium hydroxide.

[0024] Optionally, the iron source is a soluble salt containing iron; optionally, the sodium source includes at least one of ferrous sulfate, ferrous carbonate, and ferrous oxalate.

[0025] Optionally, the sulfur source is a soluble sulfur-containing salt; optionally, the sulfur source includes at least one of ferrous sulfate, sodium sulfate, and potassium sulfate.

[0026] The present invention provides a sodium iron sulfate positive electrode material prepared by the preparation method.

[0027] The present invention also provides an application of the sodium iron sulfate positive electrode material in a sodium ion battery. Typically, but not limitedly, the sodium ion battery can be assembled in a manner as follows: the sodium iron sulfate positive electrode material is mixed evenly with the conductive agent acetylene carbon black and the binder PVDF (polytetrafluoroethylene) in a mass ratio of 80:10:10, and an appropriate amount of 1-methyl-2-pyrrolidone is added and ball-milled for 1 hour to form a slurry, which is evenly coated on an aluminum sheet, and then dried and pressed into a positive electrode sheet with a compaction density of 2.0 g / cm 3 , using 1 mol / L NaClO4 PC (propylene carbonate) solution as the electrolyte and a metal sodium sheet as the negative electrode to assemble a 2032 button battery.

[0028] The beneficial effects of the present invention are: The present invention provides a method for preparing a sodium ferric sulfate positive electrode material, comprising the following steps: S1: mixing a sodium source, an iron source, a sulfur source, an antioxidant, an organic carbon source, an inorganic carbon source, a dispersant, a defoaming agent, and deionized water to obtain a suspension; S2: spray drying the suspension obtained in S1 to obtain a sodium ferric sulfate positive electrode material precursor; S3: sintering the sodium ferric sulfate positive electrode material precursor obtained in S2 to obtain a sodium ferric sulfate positive electrode material. The surface of the sodium ferric sulfate positive electrode material obtained by the preparation method has a uniform carbon coating layer, which can be used as a protective barrier layer to effectively isolate moisture and carbon dioxide in the air, and will not have defect sites. It can improve the air stability of the sodium ferric sulfate positive electrode material, and provide the sodium ferric sulfate positive electrode material with the ability to be stored in a long-term natural environment and excellent electrochemical properties, such as higher conductivity. The uniform carbon coating layer formed can also enhance the conductivity between particles, reduce battery polarization, and inhibit the growth of grains, thereby refining the grains and shortening the Na + The diffusion path inside the particles improves charge transfer and further enhances the electrochemical performance of the positive electrode material. The organic carbon source and inorganic carbon source evenly distributed in the suspension can form a coating layer with consistent carbon content on the surface of the sodium ferric sulfate material after spray drying and sintering. The combined use of dispersants and defoamers can evenly distribute the organic carbon source and inorganic carbon source in the suspension to ensure the uniformity of the carbon content in the suspension; the addition of dispersants effectively avoids the agglomeration of inorganic carbon sources in the suspension; the addition of defoamers can remove the foam generated by the addition of dispersants, avoiding the uneven distribution of carbon content in the suspension caused by foam. DETAILED DESCRIPTION

[0029] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0030] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0031] Example 1 This embodiment provides a sodium iron sulfate positive electrode material and a preparation method thereof, comprising the following steps: (1) Take Na2SO4 and FeSO4·7H2O in a molar ratio of 1:1.2, and continue to take 5% of the mass of an organic carbon source (glucose), 4% of the mass of an inorganic carbon source (acetylene black), 2% of the mass of an antioxidant (ascorbic acid), 1% of the mass of a dispersant (sodium dodecyl sulfate), and 50 ppm of the mass of a defoaming agent (hydroxymethyl cellulose); add deionized water to a stirrer reactor, add all the above reagents to the stirrer reactor, set the stirrer speed to 200 r / min, stir for 2 h, so that all the reagents except the inorganic carbon source are fully dissolved, and finally obtain a suspension with a solid content of 25%.

[0032] (2) The suspension obtained in (1) is subjected to spray drying treatment, wherein the inlet air temperature of the spray drying is 200° C. and the outlet air temperature is 100° C., to obtain a sodium iron sulfate positive electrode material precursor.

[0033] (3) The sodium iron sulfate cathode material precursor obtained in (2) was transferred to a box furnace, and under a nitrogen atmosphere, the temperature was first raised to 200°C and sintered for 6 hours, and then continued to be raised to 370°C and sintered for 12 hours to obtain a sodium iron sulfate cathode material with a chemical formula of Na 2.72 Fe 1.64 (SO4)3.

[0034] Example 2 This embodiment provides a sodium iron sulfate positive electrode material and a preparation method thereof, comprising the following steps: (1) Take Na2SO4 and FeSO4·7H2O in a molar ratio of 1:1.2, and continue to take their mass and 0.01% of organic carbon source (fructose), their mass and 6% of inorganic carbon source (activated carbon), their mass and 0.05% of antioxidant (citric acid), their mass and 5% of dispersant (sodium alkylbenzene sulfonate), their mass and 100ppm of defoaming agent (hydroxymethyl cellulose); add deionized water to a stirrer reactor, add all the above reagents into the stirrer reactor, set the stirrer speed to 400r / min, stir for 2h, so that all reagents except the inorganic carbon source are fully dissolved, and finally obtain a suspension with a solid content of 40%.

[0035] (2) The suspension obtained in (1) was spray dried at an air inlet temperature of 280° C. and an air outlet temperature of 140° C. to obtain a sodium iron sulfate positive electrode material precursor.

[0036] (3) The sodium iron sulfate cathode material precursor obtained in (2) was transferred to a box furnace, and in an argon protective atmosphere, the temperature was first raised to 100°C and sintered for 12 h, and then further raised to 400°C and sintered for 0.1 h to obtain a sodium iron sulfate cathode material, whose chemical formula is Na 2.72 Fe 1.64 (SO4)3.

[0037] Example 3 This embodiment provides a sodium iron sulfate positive electrode material and a preparation method thereof, comprising the following steps: (1) Take Na2SO4 and FeSO4·7H2O in a molar ratio of 1:1.2, and then take 10% of the mass of an organic carbon source (sucrose), 0.05% of the mass of an inorganic carbon source (conductive carbon black), 5% of the mass of an antioxidant (oxalic acid), 0.1% of the mass of a dispersant (sodium stearate), and 1 ppm of the mass of a defoaming agent (hydroxymethyl cellulose); add deionized water to a stirrer reactor, add all the above reagents to the stirrer reactor, set the stirrer speed to 100 r / min, stir for 3 h, so that all the reagents except the inorganic carbon source are fully dissolved, and finally obtain a suspension with a solid content of 15%.

[0038] (2) The suspension obtained in (1) was spray dried at an air inlet temperature of 140° C. and an air outlet temperature of 70° C. to obtain a sodium iron sulfate positive electrode material precursor.

[0039] (3) The sodium iron sulfate cathode material precursor obtained in (2) was transferred to a box furnace, and under a nitrogen atmosphere, the temperature was first raised to 280°C and sintered for 0.1 h, and then continued to be raised to 300°C and sintered for 24 h to obtain a sodium iron sulfate cathode material with a chemical formula of Na 2.72 Fe 1.64 (SO4)3.

[0040] Comparative Example 1 This comparative example provides a sodium iron sulfate positive electrode material and a preparation method thereof, which is different from Example 1 only in that no organic carbon source, inorganic carbon source, dispersant, or defoaming agent is used in step (1).

[0041] Comparative Example 2 This comparative example provides a sodium iron sulfate positive electrode material and a preparation method thereof, which is different from Example 1 only in that in step (1), no inorganic carbon source, dispersant, or defoaming agent is used, and only Na2SO4 and FeSO4·7H2O by mass and 10% of an organic carbon source (glucose) are used.

[0042] Comparative Example 3 This comparative example provides a sodium iron sulfate positive electrode material and a preparation method thereof, which is different from Example 1 only in that no organic carbon source is used in step (1), and Na2SO4 and FeSO4·7H2O by weight and 9% of an inorganic carbon source (acetylene black) are used.

[0043] Comparative Example 4 This comparative example provides a sodium iron sulfate positive electrode material and a preparation method thereof, which is different from Example 1 only in that no dispersant or defoaming agent is used in step (1).

[0044] Comparative Example 5 This comparative example provides a sodium iron sulfate positive electrode material and a preparation method thereof, which is different from Example 1 only in that no defoaming agent is used in step (1).

[0045] Test Example 1 The sodium iron sulfate positive electrode material prepared in the embodiment and the comparative example was mixed with the conductive agent acetylene carbon black and the binder PVDF in a mass ratio of 80:10:10, and an appropriate amount of 1-methyl-2-pyrrolidone was added and ball-milled for 1 hour to form a slurry, which was evenly coated on an aluminum sheet, dried, and pressed into a positive electrode sheet with a compaction density of 2.0 g / cm 3 , using 1mol / L NaClO4 PC (propylene carbonate) solution as the electrolyte, and using metal sodium sheet as the negative electrode to assemble 2032 button batteries, the Siken test system was used for electrical performance testing. In the charge and discharge cut-off voltage range of 2.0~4.0V, the discharge specific capacity at 0.1C was tested. Rate performance test: The charge and discharge cut-off voltage was 2.0~4.5V, and the discharge capacity C1 under 1C conditions and the discharge capacity C2 under 0.1C conditions were tested, and the rate performance was C1 / C2. High temperature cycle performance test: At 40℃, in the cut-off voltage range of 2.0~4.0V, the charge and discharge rate was tested to be 1C, and the number of cycles was 50. The test results are shown in Table 1.

[0046] Test Example 2 The sodium iron sulfate positive electrode materials prepared in the embodiment and the comparative example were subjected to conductivity detection. The conductivity detection method was carried out in accordance with the "Test Method for Conductivity of Lithium Ion Battery Electrode Materials" (standard number SJ / T 11792-2022). The test results are shown in Table 1.

[0047] Test Example 3 The sodium iron sulfate positive electrode materials prepared in the embodiment and the comparative example were placed in an environment with a humidity of 20%, and samples were taken at 0h and 72h, respectively. The moisture content was determined by the Karl Fischer-Coulomb method. The test results are shown in Table 1.

[0048] Table 1

[0049] As can be seen from Table 1, the sodium iron sulfate cathode material obtained by the preparation method provided by the present application in the embodiment is significantly better than the sodium iron sulfate cathode material obtained in the comparative example in terms of initial charge and discharge specific capacity, rate performance, cycle capacity retention rate, conductivity, and water content. In the comparative example, the comparative example 1 without carbon coating has the worst effect; only an organic carbon source is used in comparative example 2, and only an inorganic carbon source is used in comparative example 3. The performance of the obtained sodium iron sulfate cathode material is better than that without carbon coating, but it is still far worse than the material obtained in the embodiment. In comparative examples 4 and 5, both an organic carbon source and an inorganic carbon source are used, but no dispersant or defoamer is added in comparative example 4, and no defoamer is added in comparative example 5. Without the help of additives, the organic carbon source and the inorganic carbon source cannot achieve uniform coating of the material, which ultimately leads to its various performances being worse than the sodium iron sulfate cathode material obtained in the embodiment. The sodium ferric sulfate positive electrode material prepared by the method for preparing the sodium ferric sulfate positive electrode material provided in the present application has a uniform carbon coating layer, excellent electrical properties, and is not easy to absorb water.

[0050] Obviously, the above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the protection scope of the invention.

Claims

1. A method for preparing a sodium iron sulfate positive electrode material, It is characterized in that The steps include: S1: Mixing a sodium source, an iron source, a sulfur source, an antioxidant, an organic carbon source, an inorganic carbon source, a dispersant, a defoaming agent, and deionized water to obtain a suspension; S2: spray drying the suspension obtained in S1 to obtain a sodium iron sulfate positive electrode material precursor; S3: Sintering the sodium iron sulfate positive electrode material precursor obtained in S2 to obtain the sodium iron sulfate positive electrode material.

2. The preparation method according to claim 1, It is characterized in that The mass of the organic carbon source is 0.01% to 10% of the sum of the mass of the sodium source, the iron source and the sulfur source; And / or, the mass of the inorganic carbon source is 0.05% to 6% of the sum of the masses of the sodium source, the iron source and the sulfur source.

3. The preparation method according to claim 1 or 2, It is characterized in that The mass of the antioxidant is 0.05% to 5% of the sum of the mass of the sodium source, the iron source and the sulfur source; And / or, the mass of the dispersant is 0.1% to 5% of the sum of the mass of the sodium source, the iron source and the sulfur source; And / or, the mass of the defoaming agent is 1-100 ppm of the sum of the mass of the sodium source, the iron source and the sulfur source; And / or, the amount of sodium source, iron source and sulfur source is calculated according to the stoichiometric ratio of sodium ferric sulfate; Optionally, the sodium ferric sulfate is a non-stoichiometric sodium ferric sulfate; Optionally, the chemical formula of the non-stoichiometric sodium ferric sulfate is Na x Fe y (SO 4 ) z , where 2≤x≤3, 1.5≤y≤2, 1≤x / y≤2, x+2y=2z.

4. The preparation method according to any one of claims 1 to 3, It is characterized in that The mass of the deionized water is 15% to 40% of the sum of the mass of the sodium source, the iron source, the sulfur source, the antioxidant, the organic carbon source, the inorganic carbon source, the dispersant, and the defoaming agent.

5. The preparation method according to any one of claims 1 to 4, It is characterized in that In step S2, the inlet air temperature of the spray drying is 140-280°C, and the outlet air temperature is 70-140°C.

6. The preparation method according to any one of claims 1 to 5, It is characterized in that In the step S3, the sintering includes a first stage sintering and a second stage sintering, the first stage sintering is performed at a temperature of 100-280°C and a time of 0.1-12 hours, and the second stage sintering is performed at a temperature of 300-400°C and a time of 0.1-24 hours.

7. The preparation method according to any one of claims 1 to 6, It is characterized in that In the step S1, after mixing, a stirring step is further included, the stirring speed is 100-400 r / min, and the stirring time is 2-3 h; And / or, in step S3, sintering is performed under nitrogen and / or inert gas atmosphere; And / or, in the step S3, the step of crushing the sintering material is also included after sintering.

8. The preparation method according to any one of claims 1 to 7, It is characterized in that The organic carbon source is a water-soluble organic carbon source; optionally, the organic carbon source includes at least one of glucose, sucrose, fructose, and water-soluble starch; And / or, the inorganic carbon source includes at least one of acetylene black, graphene, carbon nanotubes, carbon fibers, activated carbon, and conductive carbon black; And / or, the dispersant includes at least one of sodium lauryl sulfate, polyethylene glycol, sodium alkylbenzene sulfonate, sodium alkyl sulfonate, sodium stearate, and polyvinyl pyrrolidone; And / or, the defoaming agent includes at least one of hydroxymethyl cellulose, polysiloxane, and polyether-modified silicone oil; And / or, the antioxidant is a water-soluble antioxidant; optionally, the antioxidant includes at least one of ascorbic acid, citric acid, phytic acid, uric acid, oxalic acid, formic acid, and acetic acid; And / or, the sodium source is a soluble salt containing sodium; optionally, the sodium source includes at least one of sodium sulfate, sodium bisulfate, sodium carbonate, sodium bicarbonate, sodium nitrate, and sodium hydroxide; And / or, the iron source is a soluble salt containing iron; optionally, the sodium source includes at least one of ferrous sulfate, ferrous carbonate, and ferrous oxalate; And / or, the sulfur source is a soluble salt containing sulfur; optionally, the sulfur source includes at least one of ferrous sulfate, sodium sulfate and potassium sulfate.

9. A sodium iron sulfate positive electrode material prepared by the preparation method as described in any one of 1 to 8.

10. Use of the sodium iron sulfate positive electrode material as claimed in claim 9 in a sodium ion battery.

Citation Information

Cited By

  • Novel sodium iron silicate sulfate composite polyanion positive electrode material for sodium-ion battery and preparation method of novel sodium iron silicate sulfate composite polyanion positive electrode material

    CN119695149A

  • Composite carbon-coated sodium ferrous sulfate positive electrode material as well as preparation method and application thereof

    CN120413642A

  • Sodium-ion battery positive electrode material and preparation method thereof

    CN120914224A

  • Preparation method and application of composite graphene carbon material coated sodium ferric sulfate material

    CN121342092A