A high-strength composite material based on polypropylene and preparation method thereof

By using surface graft modified jute fibers and flame retardant synergist in polypropylene composites, the problem of insufficient strength and flame retardant performance of polypropylene composites is solved, and a combination of high strength and excellent flame retardant performance is achieved. Improves the safety and reliability of the material.

CN118725461BActive Publication Date: 2024-11-26JIANGXI BENXIAOXIONG ENVIRONMENTAL PROTECTION MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411231817.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-26
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

Existing polypropylene composites have shortcomings in strength and flame retardant properties, especially the poor compatibility of barium sulfate masterbatches and glass fibers and the lack of flame retardant functions, which limit their application range.

Method used

Modified jute fibers with ended hydroxy polyethersulfone and flame retardant synergist are used to improve the dispersion of fibers in the polypropylene matrix through ultrasonic dispersion and chemical modification, and dense expansion is formed through materials such as guar gum. Carbon layer structure to enhance flame retardant properties.

Benefits of technology

It significantly improves the mechanical strength and flame retardant properties of polypropylene composite materials, avoids the risk of rupture and fire of plastic products under external forces, extends the service life and reduces the destructiveness of fire.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725461B_ABST
    Figure CN118725461B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of composite materials, and discloses a high-strength composite material based on polypropylene and a preparation method thereof. The composite material comprises the following raw materials: polypropylene, maleic anhydride grafted polypropylene, a reinforcing filler, a flame retardant synergist, titanium dioxide, a plasticizer, an antioxidant, and a lubricant; wherein the reinforcing filler is obtained by chemically connecting jute fiber with hydroxyl-terminated polyether sulfone, and utilizing the excellent mechanical properties and rigid benzene ring structure of the jute fiber in the reinforcing filler to effectively enhance the mechanical strength of the polypropylene composite material; the flame retardant synergist is obtained by introducing a nitrogen-phosphorus flame retardant into the structure of guar gum, thereby improving the flame retardant performance of the polypropylene composite material, reducing the destructiveness of fire and the risk of casualties, and being conducive to improving the service life of the polypropylene composite material and its products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, and in particular to a high-strength composite material based on polypropylene and a preparation method thereof. Background Art

[0002] Polypropylene has the advantages of light weight, non-toxicity, good insulation, easy processing and corrosion resistance. It is one of the most widely used general-purpose plastics. With the continuous acceleration of urbanization, plastic products made from polypropylene as raw material have shown great application prospects in all walks of life.

[0003] With the development demand of diversification and functionalization of plastic products, higher requirements are put forward for polypropylene materials. Polypropylene materials need to withstand various external forces and stresses during use. Therefore, polypropylene composite materials need to have high strength performance to ensure that plastic products can maintain structural integrity when subjected to external forces, thereby avoiding plastic products from breaking or being damaged during use, and improving the safety and reliability of plastic products. Secondly, polypropylene is a flammable material. When burning, it is easy to release a lot of heat accompanied by molten droplets, which can easily cause fires and pose a serious threat to people’s lives and property safety, thereby limiting the application scope of plastic products. Therefore, it is particularly important to flame retardantly modify polypropylene.

[0004] In the prior art, the improvement of the performance of polypropylene materials is mostly achieved by filling and modifying the strength, flame retardancy and other properties of polypropylene materials. For example, the invention patent with the publication number CN103540018B discloses a high-strength polypropylene composite material and its preparation method. The invention modifies the polypropylene matrix by adding a mineral reinforcing agent barium sulfate masterbatch and a fiber reinforcing agent glass fiber at the same time, and supplemented with other additives, so that the prepared polypropylene composite material has excellent gloss, mechanical strength, shrinkage and good dimensional stability. However, the use of additives such as minerals and fibers can effectively enhance the strength of the polypropylene composite material, but the compatibility between the barium sulfate masterbatch and the glass fiber and the polypropylene matrix is ​​poor, and the polypropylene composite material does not have the flame retardant function, and there are still defects in actual production. Based on this, it is of great significance for the present invention to prepare a polypropylene composite material with excellent flame retardancy and mechanical strength. Summary of the invention

[0005] In order to solve the problems mentioned in the background technology, the object of the present invention is to provide a high-strength composite material based on polypropylene and a preparation method thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A high-strength composite material based on polypropylene comprises the following raw materials in parts by weight: 60 to 80 parts of polypropylene, 5 to 15 parts of maleic anhydride grafted polypropylene, 5 to 10 parts of reinforcing fillers, 4 to 8 parts of flame retardant synergists, 8 to 10 parts of titanium dioxide, 1 to 3 parts of plasticizers, 1 to 2 parts of antioxidants, and 0.5 to 1.5 parts of lubricants.

[0008] Furthermore, the preparation method of the reinforcing filler comprises the following steps:

[0009] A1: Ultrasonic dispersion of jute fiber in N,N-dimethylformamide solution, nitrogen protection, adding chloromethyldichloromethylsilane and promoting agent, mixing, raising the system temperature to 50-70°C, keeping stirring at this temperature for 3-5 hours, collecting solid materials, washing, and vacuum drying to obtain modified jute fiber;

[0010] A2: Add modified jute fiber and ethanol to a nitrogen-protected reactor, stir evenly, then add hydroxy-terminated polyethersulfone and sodium carbonate. After the addition is complete, turn on the heating until the temperature in the reactor reaches 60-70°C. After keeping warm and stirring for 3-6 hours, filter the material, take a solid sample, wash the sample with deionized water, and dry it to obtain a reinforcing filler.

[0011] Furthermore, in step A1, the jute fiber has a diameter of 2 to 10 μm and a length of 1 to 4 mm.

[0012] Furthermore, in step A1, the promoting auxiliary agent is any one of pyridine or triethylamine.

[0013] Furthermore, in step A2, the weight average molecular weight of the hydroxy-terminated polyethersulfone is 1000 to 5000.

[0014] Furthermore, the preparation method of the flame retardant synergist comprises the following steps:

[0015] AA1: Place guar gum in a toluene solution, ultrasonically disperse for 10 to 30 minutes, pass nitrogen, exhaust the air, add iminodiacetic acid and a catalyst, stir and disperse evenly, raise the temperature to 90 to 110°C, keep stirring for 4 to 6 hours, wait for the material to cool naturally, and discharge the material to obtain modified guar gum;

[0016] AA2: Under nitrogen protection, add modified guar gum to dimethyl sulfoxide solution, stir mechanically, add tri(2-chloroethyl) phosphate and potassium hydroxide, raise the system temperature to 40-60°C under stirring conditions, keep warm for 4-8 hours, stop heating and remove nitrogen, cool to room temperature and then discharge to obtain a flame retardant synergist.

[0017] Furthermore, in step AA1, the catalyst is any one of p-toluenesulfonic acid, aminosulfonic acid or trifluoromethanesulfonic acid.

[0018] Furthermore, in step AA1, the mass ratio of the guar gum to the iminodiacetic acid is 1:0.1-0.3.

[0019] Furthermore, the plasticizer is any one of dibutyl phthalate, dioctyl phthalate or diisodecyl phthalate; the antioxidant is any one of antioxidant 1076, antioxidant 168 or antioxidant 2246; and the lubricant is any one of paraffin wax or polyethylene wax.

[0020] A method for preparing a high-strength composite material based on polypropylene comprises the following steps:

[0021] (1) Adding polypropylene, maleic anhydride grafted polypropylene, reinforcing filler, flame retardant synergist, titanium dioxide, plasticizer, antioxidant and lubricant into a mixer, stirring and mixing at a speed of 500 to 700 r / min for 20 to 40 minutes, discharging the materials, and obtaining a premix;

[0022] (2) The premix obtained in step (1) is put into a twin-screw extruder, the speed of the extruder is set to 300-500 r / min, the melting temperature is set to 190-210° C., and melt extrusion granulation is performed to obtain a polypropylene composite material.

[0023] Beneficial effects of the present invention:

[0024] (1) The reinforcing filler prepared by the present invention is jute fiber with end-hydroxyl polyether sulfone grafted on the surface. After being organically modified, the dispersibility of the jute fiber in the polypropylene matrix is ​​improved, so that it is not easy to agglomerate during use. On the one hand, the rigid benzene ring structure on the surface of the jute fiber can effectively enhance the mechanical strength of the polypropylene composite material, realize the reinforcement of the polypropylene, and is beneficial to improve the service life of the polypropylene composite material and its products. On the other hand, the excellent mechanical properties of the jute fiber itself can be utilized to produce synergy with the rigid benzene ring structure to avoid the problem of plastic products being broken or damaged when subjected to external forces, thereby further enhancing the mechanical strength of the polypropylene composite material. In addition, the silicon element in the reinforcing filler structure can produce a synergistic flame retardant effect with the flame retardant synergist, thereby improving the flame retardant properties of the polypropylene composite material.

[0025] (2) The present invention prepares a flame retardant synergist to perform flame retardant modification on the polypropylene composite material. The guar gum in the flame retardant synergist structure can be used as a carbon source. During the combustion process, a dense expanded carbon layer structure can be quickly formed to effectively block oxygen and heat and prevent further combustion. At the same time, the nitrogen-phosphorus flame retardant introduced into the guar gum structure can generate non-combustible gases such as nitrogen and ammonia when the polypropylene composite material is burned, as well as phosphoric acid derivatives that can promote the rapid dehydration of the polypropylene composite material, thereby producing a synergistic flame retardant effect, thereby enhancing the flame retardant properties of the polypropylene composite material and reducing the destructiveness of the fire and the risk of casualties. In addition, during the melt blending process, groups such as hydroxyl groups in the flame retardant synergist structure can interact with the maleic anhydride grafted polypropylene in the matrix to increase the crosslinking density of the polypropylene composite material, thereby making the prepared polypropylene composite material exhibit excellent mechanical strength and achieving the purpose of fixing the flame retardant in the polypropylene material.

[0026] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0028] Figure 1 This is a scanning electron microscope image of the jute fiber and reinforcing filler prepared in the present invention.

[0029] Figure 2 This is an infrared spectrum test diagram of the modified guar gum and flame retardant synergist prepared in the present invention. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The reinforcing fillers and flame retardant synergists in the examples and comparative examples of the present invention are prepared by the following method:

[0032] 1. Preparation of reinforcing fillers

[0033] A1: 5 g of jute fiber with a diameter of 4 μm and a length of 2 mm was ultrasonically dispersed in N,N-dimethylformamide solution, nitrogen was passed through, 1.4 g of chloromethyldichloromethylsilane and 0.05 g of pyridine were added, and after mixing, the system temperature was raised to 60°C, and stirred at this temperature for 4 h, the solid material was collected, washed, and vacuum dried to obtain modified jute fiber;

[0034] A2: Add 5 g of modified jute fiber and ethanol into a nitrogen-protected reactor, stir evenly, then add 2.6 g of hydroxy-terminated polyethersulfone with a weight average molecular weight of 2000 and 0.1 g of sodium carbonate. After the addition, turn on the heating until the temperature in the reactor reaches 65°C. After keeping warm and stirring for 5 hours, filter the material, take a solid sample, wash the sample with deionized water, and dry it to obtain a reinforcing filler.

[0035] The morphology of jute fiber and reinforcing filler was analyzed using a JSM-5900LV scanning electron microscope. The test results are shown in Figure 1 ,It can be observed from the figure that the jute fiber surface is smooth, while the reinforcing filler presents a rough surface morphology, which is caused by grafting ,hydroxy-terminated polyether sulfone onto the jute fiber surface.

[0036] It can be inferred that the principle of the above scheme is: under the action of pyridine, the hydroxyl groups on the surface of the jute fiber can react with the silicon-chlorine groups in the structure of chloromethyldichloromethylsilane, thereby modifying the halogen groups on the surface of the jute fiber to obtain modified jute fiber; under the action of sodium carbonate, the hydroxyl groups in the structure of the terminal hydroxyl polyethersulfone can react with the halogen groups on the surface of the modified jute fiber, thereby grafting the terminal hydroxyl polyethersulfone to the surface of the jute fiber to obtain a reinforcing filler.

[0037] 2. Preparation of flame retardant synergist

[0038] AA1: 6 g of guar gum was placed in a toluene solution, and ultrasonically dispersed for 20 min. After nitrogen was passed and the air was exhausted, 1.6 g of iminodiacetic acid and 0.1 g of p-toluenesulfonic acid were added, and the mixture was stirred and dispersed evenly. The temperature was raised to 100 ° C, and the mixture was stirred and kept warm for 5 h. After the material was cooled naturally, the modified guar gum was obtained.

[0039] AA2: Under nitrogen protection, add 6 g of modified guar gum to dimethyl sulfoxide solution, stir mechanically, add 1.2 g of tri(2-chloroethyl) phosphate and 0.08 g of potassium hydroxide, raise the system temperature to 50°C under stirring conditions, keep warm for 6 hours, stop heating and remove nitrogen, cool to room temperature and then discharge to obtain a flame retardant synergist.

[0040] The modified guar gum and flame retardant synergist were analyzed by infrared spectroscopy using Spectrum Two infrared spectrometer. The analysis results are shown in Figure 2 ,Depend on Figure 2 It can be seen that in the infrared spectrum of modified guar gum, The absorption peak of the ester group C=O appears at The absorption peak of ether bond COC appears at The absorption peak of CN appears at The absorption peak of NH appears at ; in the infrared spectrum of the flame retardant synergist, The absorption peak of the ester group C=O appears at The absorption peak of ether bond COC appears at The absorption peak of P=O appears at The absorption peak of CN appears at , the absorption peak of CN is enhanced, and the absorption peak of NH disappears.

[0041] It can be inferred that the principle of the above scheme is: the guar gum structure contains active hydroxyl groups, which can undergo esterification reaction with the carboxyl groups in the iminodiacetic acid structure under the action of p-toluenesulfonic acid, thereby introducing imino groups into the structure of guar gum to obtain modified guar gum. Under the action of potassium hydroxide, the imino groups in the modified guar gum structure can react with the halogen groups in the tris(2-chloroethyl) phosphate structure, so that the guar gum and tris(2-chloroethyl) phosphate are chemically bonded to obtain a flame retardant synergist. Example 1

[0042] Preparation of polypropylene composite materials

[0043] (1) Add 60 g of polypropylene, 5 g of maleic anhydride grafted polypropylene, 5 g of reinforcing filler, 4 g of flame retardant synergist, 8 g of titanium dioxide, 1 g of dioctyl phthalate, 1 g of antioxidant 168 and 0.5 g of polyethylene wax into a mixer, stir and mix at a speed of 500 r / min for 20 min, and discharge to obtain a premix;

[0044] (2) The premix obtained in step (1) is put into a twin-screw extruder, the speed of the extruder is set to 300 r / min, the melting temperature is set to 190° C., and melt extrusion granulation is performed to obtain a polypropylene composite material. Example 2

[0045] Preparation of polypropylene composite materials

[0046] (1) Add 70 g of polypropylene, 10 g of maleic anhydride grafted polypropylene, 8 g of reinforcing filler, 6 g of flame retardant synergist, 9 g of titanium dioxide, 2 g of dioctyl phthalate, 1.5 g of antioxidant 168 and 1 g of polyethylene wax into a mixer, stir and mix at a speed of 600 r / min for 30 min, and discharge to obtain a premix;

[0047] (2) The premix obtained in step (1) is put into a twin-screw extruder, the speed of the extruder is set to 400 r / min, the melting temperature is set to 200° C., and melt extrusion granulation is performed to obtain a polypropylene composite material. Example 3

[0048] Preparation of polypropylene composite materials

[0049] (1) Add 80 g of polypropylene, 15 g of maleic anhydride grafted polypropylene, 10 g of reinforcing filler, 8 g of flame retardant synergist, 10 g of titanium dioxide, 3 g of dioctyl phthalate, 2 g of antioxidant 168 and 1.5 g of polyethylene wax into a mixer, stir and mix at a speed of 700 r / min for 40 min, and discharge to obtain a premix;

[0050] (2) The premix obtained in step (1) is put into a twin-screw extruder, the speed of the extruder is set to 500 r / min, the melting temperature is set to 210° C., and melt extrusion granulation is performed to obtain a polypropylene composite material.

[0051] Comparative Example 1

[0052] Preparation of polypropylene composite materials

[0053] (1) Add 70 g of polypropylene, 10 g of maleic anhydride grafted polypropylene, 8 g of reinforcing filler, 9 g of titanium dioxide, 2 g of dioctyl phthalate, 1.5 g of antioxidant 168 and 1 g of polyethylene wax into a mixer, stir and mix at a speed of 600 r / min for 30 min, and discharge the mixture to obtain a premix;

[0054] (2) The premix obtained in step (1) is put into a twin-screw extruder, the speed of the extruder is set to 400 r / min, the melting temperature is set to 200° C., and melt extrusion granulation is performed to obtain a polypropylene composite material.

[0055] Comparative Example 2

[0056] Preparation of polypropylene composite materials

[0057] (1) Add 70 g of polypropylene, 10 g of maleic anhydride grafted polypropylene, 6 g of flame retardant synergist, 9 g of titanium dioxide, 2 g of dioctyl phthalate, 1.5 g of antioxidant 168 and 1 g of polyethylene wax into a mixer, stir and mix at a speed of 600 r / min for 30 min, and discharge to obtain a premix;

[0058] (2) The premix obtained in step (1) is put into a twin-screw extruder, the speed of the extruder is set to 400 r / min, the melting temperature is set to 200° C., and melt extrusion granulation is performed to obtain a polypropylene composite material.

[0059] Comparative Example 3

[0060] Preparation of polypropylene composite materials

[0061] (1) Add 70 g of polypropylene, 10 g of maleic anhydride grafted polypropylene, 5 g of jute fiber, 3 g of hydroxyl-terminated polyethersulfone, 6 g of flame retardant synergist, 9 g of titanium dioxide, 2 g of dioctyl phthalate, 1.5 g of antioxidant 168 and 1 g of polyethylene wax into a mixer, stir and mix at a speed of 600 r / min for 30 min, and discharge the mixture to obtain a premix;

[0062] (2) The premix obtained in step (1) is put into a twin-screw extruder, the speed of the extruder is set to 400 r / min, the melting temperature is set to 200° C., and melt extrusion granulation is performed to obtain a polypropylene composite material.

[0063] Comparative Example 4

[0064] Preparation of polypropylene composite materials

[0065] (1) Add 70 g of polypropylene, 10 g of maleic anhydride grafted polypropylene, 9 g of titanium dioxide, 2 g of dioctyl phthalate, 1.5 g of antioxidant 168 and 1 g of polyethylene wax into a mixer, stir and mix at a speed of 600 r / min for 30 min, and discharge the mixture to obtain a premix;

[0066] (2) The premix obtained in step (1) is put into a twin-screw extruder, the speed of the extruder is set to 400 r / min, the melting temperature is set to 200° C., and melt extrusion granulation is performed to obtain a polypropylene composite material.

[0067] Performance testing:

[0068] ① The polypropylene composite materials prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 4 were made into samples that met the test specifications, and the tensile strength of the samples was tested according to GB / T 1040.1-2018 "Determination of tensile properties of plastics Part 1: General Principles"; the impact strength of the samples was tested according to GB / T 1843-2008 "Determination of cantilever beam impact strength of plastics"; the combustion performance of the samples was tested according to GB / T 2406.2-2009 "Determination of combustion behavior of plastics by oxygen index method Part 2: Room temperature test", and the flame retardant properties of the polypropylene composite materials were evaluated. The specific test results are shown in the following table:

[0069] ;

[0070] From the test results in the above table, it can be seen that the samples prepared in Examples 1 to 3 all have excellent flame retardant properties and mechanical strength; in the sample prepared in Comparative Example 1, only reinforcing fillers were added. Compared with the examples, the limiting oxygen index value of the sample decreased significantly, the mechanical strength of the sample was good, and the flame retardant performance was poor; in the sample prepared in Comparative Example 2, no reinforcing fillers were added, so the mechanical strength was not as good as that of the examples, but since a flame retardant synergist was added therein, the limiting oxygen index of the sample was 30.6%, so the sample had excellent flame retardant properties; in the sample prepared in Comparative Example 3, jute fiber, hydroxyl-terminated polyether sulfone and flame retardant synergist were added. Compared with the examples, the flame retardant performance of the sample was good, and the mechanical strength performance was average. It is speculated that this may be because the jute fiber that has not been organically modified has agglomerated in the matrix, resulting in a decrease in the mechanical strength of the sample; in the sample prepared in Comparative Example 4, neither reinforcing fillers nor flame retardant synergists were added, so the performance of the sample was the worst.

[0071] The above contents are merely examples and explanations of the concept of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A high-strength composite material based on polypropylene, characterized in that: The invention comprises the following raw materials in parts by weight: 60 to 80 parts of polypropylene, 5 to 15 parts of maleic anhydride grafted polypropylene, 5 to 10 parts of reinforcing filler, 4 to 8 parts of flame retardant synergist, 8 to 10 parts of titanium dioxide, 1 to 3 parts of plasticizer, 1 to 2 parts of antioxidant, and 0.5 to 1.5 parts of lubricant; The preparation method of the reinforcing filler comprises the following steps: A1: Ultrasonic dispersion of jute fiber in N,N-dimethylformamide solution, nitrogen protection, adding chloromethyldichloromethylsilane and promoting agent, mixing, raising the system temperature to 50-70°C, keeping stirring at this temperature for 3-5 hours, collecting solid materials, washing, and vacuum drying to obtain modified jute fiber; A2: Add modified jute fiber and ethanol to a nitrogen-protected reactor, stir evenly, then add hydroxy-terminated polyethersulfone and sodium carbonate, and after the addition, turn on the heating until the temperature in the reactor reaches 60-70°C, keep the temperature and stir for 3-6 hours, filter the material, take a solid sample, wash the sample with deionized water, and dry it to obtain a reinforcing filler; The preparation method of the flame retardant synergist comprises the following steps: AA1: Place guar gum in a toluene solution, ultrasonically disperse for 10 to 30 minutes, pass nitrogen, exhaust the air, add iminodiacetic acid and a catalyst, stir and disperse evenly, raise the temperature to 90 to 110°C, keep stirring for 4 to 6 hours, wait for the material to cool naturally, and discharge the material to obtain modified guar gum; AA2: Under nitrogen protection, add modified guar gum to dimethyl sulfoxide solution, stir mechanically, add tri(2-chloroethyl) phosphate and potassium hydroxide, raise the system temperature to 40-60°C under stirring conditions, keep warm for 4-8 hours, stop heating and remove nitrogen, cool to room temperature and then discharge to obtain a flame retardant synergist.

2. A high-strength composite material based on polypropylene according to claim 1, characterized in that: In step A1, the jute fiber has a diameter of 2 to 10 μm and a length of 1 to 4 mm.

3. A high-strength composite material based on polypropylene according to claim 1, characterized in that: In step A1, the promoting auxiliary agent is any one of pyridine or triethylamine.

4. A high-strength composite material based on polypropylene according to claim 1, characterized in that: In step A2, the weight average molecular weight of the hydroxy-terminated polyethersulfone is 1000-5000.

5. The high-strength composite material based on polypropylene according to claim 1, characterized in that: In step AA1, the catalyst is any one of p-toluenesulfonic acid, aminosulfonic acid or trifluoromethanesulfonic acid.

6. A high-strength composite material based on polypropylene according to claim 1, characterized in that: In step AA1, the mass ratio of the guar gum to the iminodiacetic acid is 1:0.1-0.

3.

7. The high-strength composite material based on polypropylene according to claim 1, characterized in that: The plasticizer is any one of dibutyl phthalate, dioctyl phthalate or diisodecyl phthalate; the antioxidant is any one of antioxidant 1076, antioxidant 168 or antioxidant 2246; and the lubricant is any one of paraffin wax or polyethylene wax.

8. A method for preparing a high-strength composite material based on polypropylene as claimed in claim 1, characterized in that: The following steps are involved: (1) Adding polypropylene, maleic anhydride grafted polypropylene, reinforcing filler, flame retardant synergist, titanium dioxide, plasticizer, antioxidant and lubricant into a mixer, stirring and mixing at a speed of 500 to 700 r / min for 20 to 40 minutes, discharging the materials, and obtaining a premix; (2) The premix obtained in step (1) is put into a twin-screw extruder, the speed of the extruder is set to 300-500 r / min, the melting temperature is set to 190-210° C., and melt extrusion granulation is performed to obtain a polypropylene composite material.