Sample preparation method of glow discharge mass spectrometry molybdenum-based non-conductive powder sample

By mixing ultra-high-purity carbon powder and molybdenum-based non-conductive powder samples and pressing them into flakes, the problem that glow discharge mass spectrometry cannot directly analyze molybdenum-based non-conductive samples is solved, and the stability and accuracy of the detection results are achieved. It meets the analysis needs of molybdenum-based non-conductive powder samples.

CN118730650APending Publication Date: 2024-10-01JINDUICHENG MOLYBDENUM CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410728173.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Glow discharge mass spectrometry cannot directly analyze molybdenum-based non-conductive samples, resulting in inaccurate and unstable detection results, requiring complex sample preprocessing.

Method used

Ultra-high purity carbon powder and molybdenum-based non-conductive powder samples are mixed in a certain proportion, pressed into flakes, and maintained under pressure to obtain molybdenum-based non-conductive powder samples suitable for glow discharge mass spectrometers.

Benefits of technology

It improves the stability and accuracy of the detection results, meets the analysis needs of molybdenum-based non-conductive powder samples, and provides more reliable detection data.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004879358840000051
    Figure BDA0004879358840000051
  • Figure BDA0004879358840000061
    Figure BDA0004879358840000061
  • Figure BDA0004879358840000071
    Figure BDA0004879358840000071
Patent Text Reader

Abstract

The invention discloses a glow discharge mass spectrometry molybdenum-based non-conductive powder sample preparation method, which comprises: S1, uniformly mixing ultra-pure carbon powder and a molybdenum-based non-conductive powder sample according to a certain ratio to obtain a uniformly-mixed sample; and S2, pressing the uniformly mixed sample into a sheet under a certain pressure, and maintaining the pressure to obtain the molybdenum-based non-conductive powder sample suitable for the measurement of the glow discharge mass spectrometer. According to the preparation method of the glow discharge mass spectrometry molybdenum-based non-conductive powder sample, the problem that the mass spectrometry detection result of the existing glow discharge sample is inaccurate and unstable is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical element detection and analysis, and particularly relates to a method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry. Background Art

[0002] Glow discharge mass spectrometry has developed rapidly in the field of high-purity material component analysis. Generally speaking, its limit of quantification is one order of magnitude lower than that of inductively coupled plasma mass spectrometry, and it is a trace detection method, ppb level detection. Glow discharge mass spectrometry uses solid direct sampling for determination. Compared with wet chemical methods, it shortens the sample pretreatment time and also avoids the reagent and environmental pollution caused by wet chemical methods. It has obvious advantages in the rapid analysis of modern high-purity materials with multiple elements. The application of this technology in the field of high-purity metal material analysis is already very mature. However, glow discharge mass spectrometry cannot directly analyze non-conductor samples, which is a problem encountered in the actual application of this method.

[0003] Molybdenum-based non-conductive samples include ammonium paramolybdate, molybdenum dioxide and molybdenum trioxide, which are important raw materials for the production of high-purity molybdenum. Detecting the purity of molybdenum-based non-conductive samples can provide support for industrial research and production of high-purity molybdenum. Determining the content of each impurity element in molybdenum-based non-conductive samples is of great significance to the molybdenum industry. However, glow discharge mass spectrometry cannot directly analyze molybdenum-based non-conductive samples, and further sample pretreatment is required. Usually, molybdenum-based non-conductive samples use high-purity tantalum sheets as the substrate sample pool to stimulate the glow discharge of the sample. However, the preparation process of this method is easily affected by the tantalum sheet, and the preparation steps are complicated, which leads to inaccurate and unstable measurement results. Summary of the invention

[0004] The purpose of the invention is to provide a method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry, thereby solving the problem that the mass spectrometry detection results of existing glow discharge samples are inaccurate and unstable.

[0005] The technical solution adopted by the present invention is a method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry, comprising the following steps:

[0006] S1. Mix ultra-high purity carbon powder and molybdenum-based non-conductive powder sample in a certain proportion to obtain a uniformly mixed sample;

[0007] S2. Press the uniformly mixed sample into a sheet under a certain pressure and maintain the pressure to obtain a molybdenum-based non-conductive powder sample suitable for determination by a glow discharge mass spectrometer.

[0008] The present invention is also characterized in that:

[0009] The purity of the ultra-high purity carbon powder in S1 is 99.9995% to 99.9999%.

[0010] The average particle size range of the ultra-high purity carbon powder and the molybdenum-based non-conductive sample in S1 is 1 μm to 74 μm.

[0011] The weight ratio of the ultra-high purity carbon powder and the molybdenum-based non-conductive powder samples in S1 is 1 to 6:1.

[0012] The weight of the ultra-high purity carbon powder and molybdenum-based non-conductive powder sample required for a single non-conductive powder sample in S2 is 8 g to 15 g.

[0013] The pressure in S2 is 700MPa~1200Mpa.

[0014] The pressure holding time in S2 is 20s to 90s.

[0015] The beneficial effects of the present invention are:

[0016] The method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry provided by the present invention can obtain a molybdenum-based non-conductive sheet sample suitable for a glow discharge mass spectrometer. The discharge during the test is stable, which is beneficial to the stability of the glow discharge mass spectrometry test result. The test result can meet the requirements of the molybdenum-based non-conductive powder sample. DETAILED DESCRIPTION

[0017] The present invention is described in detail below in conjunction with specific implementation modes.

[0018] The method for preparing a glow discharge mass spectrometry molybdenum-based non-conductive powder sample provided by the present invention comprises the following steps:

[0019] S1. Mix ultra-high purity carbon powder and molybdenum-based non-conductive powder sample in a certain proportion to obtain a uniformly mixed sample;

[0020] The purity of ultra-high purity carbon powder is 99.9995% to 99.9999%;

[0021] The average particle size range of ultra-high purity carbon powder and molybdenum-based non-conductive samples is 1 μm to 74 μm;

[0022] The ultra-high purity carbon powder and molybdenum-based non-conductive powder samples are mixed in a weight ratio of 1 to 6:1;

[0023] S2, pressing the uniformly mixed sample into a sheet under a certain pressure, and maintaining the pressure to obtain a molybdenum-based non-conductive powder sample suitable for determination by a glow discharge mass spectrometer;

[0024] The weight of the ultra-high purity carbon powder and molybdenum-based non-conductive powder sample required for a single non-conductive powder sample is 8g to 15g;

[0025] The pressure is 700MPa~1200MPa;

[0026] The holding time is 20s to 90s.

[0027] Example 1

[0028] The method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry proposed in this embodiment comprises the following steps:

[0029] S1. Mix ultra-high purity carbon powder and molybdenum-based non-conductive powder sample in a certain proportion to obtain a uniformly mixed sample;

[0030] S2. Press the uniformly mixed sample into a sheet under a certain pressure and maintain the pressure to obtain a molybdenum-based non-conductive powder sample suitable for determination by a glow discharge mass spectrometer.

[0031] Example 2

[0032] The method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry proposed in this embodiment comprises the following steps:

[0033] S1. Mix ultra-high purity carbon powder and molybdenum-based non-conductive powder sample in a certain proportion to obtain a uniformly mixed sample;

[0034] The purity of ultra-high purity carbon powder is 99.9995% to 99.9999%;

[0035] The average particle size range of ultra-high purity carbon powder and molybdenum-based non-conductive samples is 1 μm to 74 μm;

[0036] The ultra-high purity carbon powder and molybdenum-based non-conductive powder samples are mixed in a weight ratio of 1 to 6:1;

[0037] S2, pressing the uniformly mixed sample into a sheet under a certain pressure, and maintaining the pressure to obtain a molybdenum-based non-conductive powder sample suitable for determination by a glow discharge mass spectrometer;

[0038] The weight of the ultra-high purity carbon powder and molybdenum-based non-conductive powder sample required for a single non-conductive powder sample is 8g to 15g;

[0039] The pressure is 700MPa~1200MPa;

[0040] The holding time is 20s to 90s.

[0041] Example 3

[0042] The method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry proposed in this embodiment comprises the following steps:

[0043] S1. Mix ultra-high purity carbon powder and molybdenum-based non-conductive powder sample in a certain proportion to obtain a uniformly mixed sample;

[0044] The molybdenum-based non-conductive powder is molybdenum trioxide powder; 7g of ultra-high purity carbon powder with a purity of 99.9995% and an average particle size of 10μm and 3g of molybdenum trioxide powder with an average particle size of 23μm are weighed and mixed evenly;

[0045] S2, pressing the uniformly mixed sample into a sheet under a certain pressure, and maintaining the pressure to obtain a molybdenum-based non-conductive powder sample suitable for determination by a glow discharge mass spectrometer;

[0046] The mixed powder sample was loaded into a tablet pressing mold, and the mixed sample was tableted using a tablet press. The tablet pressing parameters were a pressure of 800 MPa and a pressure holding time of 30 s, to obtain a molybdenum-based non-conductive powder sample suitable for determination by a glow discharge mass spectrometer.

[0047] Example 4

[0048] The method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry proposed in this embodiment comprises the following steps:

[0049] S1. Mix ultra-high purity carbon powder and molybdenum-based non-conductive powder sample in a certain proportion to obtain a uniformly mixed sample;

[0050] The molybdenum-based non-conductive powder is ammonium molybdate powder; 7.5 g of ultra-high purity carbon powder with a purity of 99.9995% and an average particle size of 10 μm and 2.5 g of ammonium molybdate powder with an average particle size of 50 μm are weighed and mixed evenly;

[0051] S2, pressing the uniformly mixed sample into a sheet under a certain pressure, and maintaining the pressure to obtain a molybdenum-based non-conductive powder sample suitable for determination by a glow discharge mass spectrometer;

[0052] The mixed powder sample was loaded into a tablet pressing mold, and the mixed sample was tableted using a tablet press. The tablet pressing parameters were a pressure of 700 MPa and a pressure holding time of 25 s, to obtain a molybdenum-based non-conductive powder sample suitable for determination by a glow discharge mass spectrometer.

[0053] The content of each element in the molybdenum-based non-conductive powder samples in Example 3 and Example 4 was measured using an Element GD Plus glow discharge mass spectrometer from Thermo Fisher Scientific, as shown in Table 1:

[0054] Table 1 Test sample test results control test (%)

[0055]

[0056]

[0057] As can be seen from Table 1, the content of element components in the molybdenum-based non-conductive powder sample prepared by the present invention is consistent with the standard value of the standard sample, indicating that the present invention has high accuracy and reliability.

[0058] Seven independent tests were performed on Example 3 and Example 4, respectively. The seven measurement results were statistically processed, and the precision of the present invention was evaluated based on the relative standard deviation (RSD%). The measurement results are shown in Table 2:

[0059] Table 2 Precision (n=7) %

[0060]

[0061] It can be seen from Table 2 that the RSD of each element is less than 2%, and the precision is good, which indicates that the detection result of the molybdenum-based non-conductive sample prepared by the present invention has high accuracy and good stability.

Claims

1. A method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry, characterized in that: The following steps are involved: S1. Mix ultra-high purity carbon powder and molybdenum-based non-conductive powder sample in a certain proportion to obtain a uniformly mixed sample; S2. Press the uniformly mixed sample into a sheet under a certain pressure and maintain the pressure to obtain a molybdenum-based non-conductive powder sample suitable for determination by a glow discharge mass spectrometer.

2. The method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry according to claim 1, characterized in that: The purity of the ultra-high purity carbon powder in S1 is 99.9995% to 99.9999%.

3. The method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry according to claim 1, characterized in that: The average particle size range of the ultra-high purity carbon powder and the molybdenum-based non-conductive sample described in S1 is 1 μm to 74 μm.

4. The method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry according to claim 1, characterized in that: The ultra-high purity carbon powder and the molybdenum-based non-conductive powder sample described in S1 are mixed in a weight ratio of 1 to 6:

1.

5. The method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry according to claim 1, characterized in that: The weight of the ultra-high purity carbon powder and the molybdenum-based non-conductive powder sample required for a single non-conductive powder sample in S2 is 8 g to 15 g.

6. The method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry according to claim 1, characterized in that: The pressure in S2 is 700MPa to 1200MPa.

7. The method for preparing a molybdenum-based non-conductive powder sample for glow discharge mass spectrometry according to claim 1, characterized in that: The holding time in S2 is 20s to 90s.

Citation Information

Cited By

  • Metal oxide sample wafer and preparation and detection method thereof

    CN120778460A

  • Metal oxide samples and their preparation and detection methods

    CN120778460B