Diaphragm and preparation method thereof, battery and electric equipment

By modifying the acrylic monomer polymer to form side chains in the battery separator, the problem of high battery short circuit rate and complex formulation is solved, a separator with low short circuit rate and high performance is achieved, and the risk of short circuit and production cost of the battery are reduced.

CN118738768APending Publication Date: 2024-10-01SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410738580.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Battery short circuit causes battery failure, increases manufacturing costs, and poses a safety threat of fire and smoke. Existing coating film additives increase the risk of short circuit and complicate the preparation process.

Method used

The polymer of modified acrylic monomer is used as the composite binder. By forming side chains on the acrylic monomer, the free space of the coating slurry is reduced, the use of additives is reduced, and the dispersion and adhesion are improved. Forms a diaphragm with low short circuit rate.

Benefits of technology

It can effectively reduce the battery short circuit rate, improve battery performance, shorten the slurry preparation time, and enhance the heat resistance and wettability of the separator.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004882517760000131
    Figure BDA0004882517760000131
  • Figure BDA0004882517760000141
    Figure BDA0004882517760000141
Patent Text Reader

Abstract

The invention provides a diaphragm and a preparation method thereof, a battery and electric equipment, and relates to the technical field of batteries. The diaphragm comprises a base membrane and a composite coating arranged on at least one side of the base membrane, and the composite coating comprises a coating main material and a composite binder; the composite binder is selected from a polymer of a modified acrylic monomer; the modified acrylic monomer comprises an acrylic monomer with a side chain; the side chain comprises a first branch chain, and the first branch chain is selected from at least one of carboxymethyl, hydroxyethyl and hydroxypropyl. According to the composite adhesive provided by the invention, the composite adhesive is selected from a polymer of a modified acrylic monomer, and due to the fact that the polymer of the modified acrylic monomer has the characteristics of adhesion, dispersity, wettability and the like, introduction of auxiliaries can be reduced during slurry preparation, and the risk of isolation short circuit can be reduced, so that the short circuit rate of a battery is reduced, and the service life of the battery is prolonged. Meanwhile, the preparation time of the slurry is also shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a diaphragm and a preparation method thereof, a battery and an electrical device. Background Art

[0002] Battery short circuit is one of the forms of battery failure. The harm caused by battery short circuit can cause battery voltage failure, battery failure to work properly, and increase manufacturing costs; in severe cases, the battery will catch fire and smoke, threatening the safety of life and property. Therefore, short circuits should be avoided as much as possible during the production process. As one of the battery components, the diaphragm will also affect the battery short circuit rate.

[0003] In order to improve the short circuit rate and electrical performance of the battery, power batteries often use coating films. Various additives need to be added when preparing the coating slurry of the coating film. The introduction of additives in the coating slurry will increase the risk of diaphragm short circuit, thereby increasing the risk of battery short circuit. In addition, the addition of additives increases the preparation process and time of the coating slurry. Summary of the invention

[0004] Purpose of the invention: The present invention provides a diaphragm and a method for preparing the same, which can reduce the risk of short circuit isolation, thereby reducing the short circuit rate of the battery. The present invention also provides a battery and an electrical device, which have the advantages of low short circuit rate and good performance.

[0005] The first aspect of the present application provides a diaphragm, comprising a base film and a composite coating provided on at least one side of the base film, wherein the composite coating comprises a coating main material and a composite binder; the composite binder is selected from a polymer of a modified acrylic monomer;

[0006] The modified acrylic monomer includes an acrylic monomer having a side chain;

[0007] The side chain includes a first branch chain, and the first branch chain is selected from at least one of carboxymethyl, hydroxyethyl, and hydroxypropyl.

[0008] In some embodiments, the side chain further includes a second branch chain, and the second branch chain is selected from at least one of a hyperbranched polyether, a polyether-modified siloxane, a polyether-modified acetylenic glycol, and a polyether-modified olefinic glycol.

[0009] In some embodiments, the mass ratio of the coating main material to the composite binder is 93-97:3-7.

[0010] In some embodiments, the acrylic monomer is selected from at least one of acrylic acid and methacrylic acid.

[0011] In some embodiments, the coating main material is selected from at least one of inorganic oxides, polymethyl methacrylate, polyethylene spheres, and polytetrafluoroethylene.

[0012] In some embodiments, the polymer of the modified acrylic monomer is selected from at least one of a homopolymer formed by homopolymerization of a modified acrylic monomer, a copolymer formed by copolymerization of multiple modified acrylic monomers, a copolymer formed by copolymerization of a modified acrylic monomer and acrylonitrile, and a copolymer formed by copolymerization of a modified acrylic monomer and acrylamide.

[0013] In some embodiments, the base film has a first thickness H1, and the composite coating has a second thickness H2, satisfying: 1.25≤H1 / H2≤20.

[0014] In some embodiments, the base film has a first thickness H1 that satisfies: 5 μm≤H1≤20 μm.

[0015] In some embodiments, the composite coating has a second thickness H2 that satisfies: 1 μm≤H2≤4 μm.

[0016] A second aspect of the present application provides a method for preparing a diaphragm, comprising:

[0017] Mixing the composite binder and the solvent for the first time to obtain a first mixture;

[0018] Mixing the coating main material with the first mixture for a second time to obtain a coating slurry;

[0019] Applying the coating slurry on at least one side of the base film to obtain a diaphragm;

[0020] The composite binder is selected from polymers of modified acrylic monomers;

[0021] The modified acrylic monomer includes an acrylic monomer having a side chain;

[0022] The side chain includes a first branch chain, and the first branch chain is selected from at least one of carboxymethyl, hydroxyethyl, and hydroxypropyl.

[0023] In some embodiments, the side chain further includes a second branch chain, and the second branch chain is selected from at least one of a hyperbranched polyether, a polyether-modified siloxane, a polyether-modified acetylenic glycol, and a polyether-modified olefinic glycol.

[0024] In some embodiments, the polymer of the modified acrylic monomer is selected from at least one of a homopolymer formed by homopolymerization of a modified acrylic monomer, a copolymer formed by copolymerization of multiple modified acrylic monomers, a copolymer formed by copolymerization of a modified acrylic monomer and acrylonitrile, and a copolymer formed by copolymerization of a modified acrylic monomer and acrylamide.

[0025] In some embodiments, the mass ratio of the coating main material, the composite binder and the solvent is 93-97:3-7:95-99.

[0026] In some embodiments, the first mixing time is 20 to 40 minutes.

[0027] In some embodiments, the second mixing time is 100 to 180 minutes.

[0028] A third aspect of the present application provides a battery, comprising the diaphragm as described above or a diaphragm prepared by the diaphragm preparation method as described above.

[0029] A fourth aspect of the present application provides an electrical device, comprising the battery as described above.

[0030] The present application provides a composite adhesive, which is selected from a polymer of modified acrylic monomers. The acrylic monomers are modified to form side chains on the acrylic monomers, wherein the side chains include a first branch chain, which is selected from at least one of carboxymethyl, hydroxyethyl, and hydroxypropyl. The hydrogen bonds in the first branch chain can associate with water molecules in the slurry, thereby increasing the fluid volume of the polymer itself and reducing the free activity space of the coating main material in the coating slurry, so that the coating slurry can achieve an anti-settling effect. At the same time, the branch chain is easy to ionize positively charged hydrogen ions, and the coating slurry prepared under the repulsion of like charges has good dispersibility. Since the polymer of the modified acrylic monomer has the characteristics of adhesion, dispersibility, wettability, etc., the introduction of auxiliary agents can be reduced when preparing the slurry, the risk of isolation short circuit can be reduced, thereby reducing the short circuit rate of the battery, and the preparation time of the slurry is also shortened.

[0031] The present application provides a battery and an electrical device, including the diaphragm as described above or a diaphragm prepared by the diaphragm preparation method as described above, which has the advantages of low short circuit rate and good performance. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the embodiments of the present application. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.

[0033] In the present specification, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the minimum value and the maximum value, respectively.

[0034] The first aspect of the present application provides a diaphragm, and the present application will be described in detail below in conjunction with specific embodiments.

[0035] A diaphragm comprises a base film and a composite coating arranged on at least one side of the base film, wherein the composite coating comprises a coating main material and a composite adhesive; the composite adhesive is selected from a polymer of modified acrylic monomers; the modified acrylic monomers include acrylic monomers with side chains; the side chains include a first branch chain, and the first branch chain is selected from at least one of carboxymethyl, hydroxyethyl, and hydroxypropyl.

[0036] It can be understood that the polymer of acrylic monomers has an adhesive effect, which can achieve the bonding of the composite coating to the base film, and is not easy to separate. The present application provides a composite adhesive, which is selected from the polymer of modified acrylic monomers. The acrylic monomers are modified to form side chains on the acrylic monomers. The side chains include a first branch chain, and the first branch chain is selected from at least one of carboxymethyl, hydroxyethyl, and hydroxypropyl. The hydrogen bonds in the first branch chain can associate with water molecules in the slurry, increase the fluid volume of the polymer itself, and reduce the free activity space of the coating main material in the coating slurry, so that the coating slurry can achieve an anti-settling effect. At the same time, the branch chain is easy to ionize positively charged hydrogen ions, and the coating slurry prepared under the repulsion of like charges has good dispersibility; because the polymer of modified acrylic monomers has the characteristics of adhesion, dispersibility, wettability, etc., the introduction of additives can be reduced when preparing the slurry, the risk of isolation short circuit can be reduced, thereby reducing the short circuit rate of the battery, and the preparation time of the slurry is also shortened.

[0037] In some embodiments, the side chain further includes a second branch chain, and the second branch chain is selected from at least one of a hyperbranched polyether, a polyether-modified siloxane, a polyether-modified acetylenic glycol, and a polyether-modified olefinic glycol.

[0038] It can be understood that the present application provides a composite adhesive, the composite adhesive is selected from a polymer of modified acrylic monomers, and the acrylic monomers are modified to form side chains on the acrylic monomers, the side chains include a first branch chain and a second branch chain, the first branch chain is selected from at least one of carboxymethyl, hydroxyethyl, and hydroxypropyl, the hydrogen bonds in the first branch chain can associate with water molecules in the slurry, increase the fluid volume of the polymer itself, reduce the free activity space of the coating main material in the coating slurry, and make the coating slurry achieve an anti-settling effect, and at the same time, the branch chain is easy to ionize positively charged hydrogen ions, and under the repulsion of like charges, the coating in the coating slurry can be The coating main material is evenly dispersed to avoid black spots on the surface of the diaphragm due to agglomeration of the coating main material after coating; the second branch chain is selected from at least one of hyperbranched polyether, polyether-modified siloxane, polyether-modified acetylene glycol, and polyether-modified ethylene glycol. The second branch chain has a strong polarity, which can reduce the surface energy of the base film, so that the coating slurry can be well wetted on the surface of the base film without missing any coating; because the polymer of the modified acrylic monomer has the characteristics of adhesion, dispersibility, wettability, etc., the introduction of auxiliary agents can be further reduced when preparing the slurry, which can reduce the risk of isolation short circuit, thereby reducing the short circuit rate of the battery, and also shortening the preparation time of the slurry.

[0039] In one specific embodiment, the modified acrylic monomer side chain includes a first branched chain.

[0040] In another specific embodiment, the modified acrylic monomer side chain includes a first branch chain and a second branch chain.

[0041] In some embodiments, the mass ratio of the coating main material to the composite binder is 93-97:3-7. Specifically, the mass ratio of the coating main material to the composite binder can be any one of 93:7, 94:6, 95:5, 97:3 or a range between any two of the ratios.

[0042] It can be understood that the coating main material is used to improve the heat resistance and wettability of the base film; the composite adhesive is mainly used to make the composite coating formed by the coating slurry adhere to the base film and not easy to detach, and it also has the function of dispersing the coating main material in the solvent. The present application controls the mass ratio of the coating main material and the composite adhesive to 93~97:3~7, so as to form a coating slurry with good dispersion and wettability, and the prepared diaphragm has good heat resistance and wettability.

[0043] In some embodiments, the acrylic monomer is selected from at least one of acrylic acid and methacrylic acid.

[0044] It can be understood that the polymer of acrylic monomers has an adhesive effect, which can achieve the bonding of the composite coating and the base film, and is not easy to separate. The present application provides a modified acrylic monomer, which is formed on the acrylic monomer by modifying the acrylic monomer to form a side chain, so that the polymer of the modified acrylic monomer has the characteristics of adhesion, dispersibility, wettability, etc., which can reduce the introduction of additives when preparing the slurry, reduce the risk of isolation short circuit, thereby reducing the short circuit rate of the battery, and also shorten the preparation time of the slurry.

[0045] In some embodiments, the coating main material is selected from at least one of inorganic oxides, polymethyl methacrylate, polyethylene spheres, and polytetrafluoroethylene.

[0046] It can be understood that the coating main material is used to improve the heat resistance and wettability of the base film. In the present application, by making the coating main material selected from at least one of inorganic oxides, polymethyl methacrylate, polyethylene balls, and polytetrafluoroethylene, the heat resistance and wettability of the diaphragm can be improved, while reducing the risk of isolation short circuit.

[0047] In some embodiments, the particle size of the coating main material can be 0.2-6.0 μm, and the particle size D50 of the coating slurry can be 1.5-6.0 μm. Specifically, the particle size of the coating main material can be any one of 0.2 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, and 6 μm, or a range between any two values. The particle size D50 of the coating slurry can be any one of 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, and 6 μm, or a range between any two values.

[0048] It can be understood that by controlling the particle size of the coating main material to be 0.2-6.0 μm and the particle size D50 of the coating slurry to be 1.5-6.0 μm, the coating main material is more easily dispersed in the coating slurry, and the prepared coating slurry has good dispersibility.

[0049] In some embodiments, the inorganic oxide is selected from at least one of alumina, boehmite, magnesium oxide, silicon oxide, and aluminum hydroxide.

[0050] In some embodiments, the polymer of the modified acrylic monomer includes at least one of a homopolymer formed by homopolymerization of a modified acrylic monomer, a copolymer formed by copolymerization of multiple modified acrylic monomers, a copolymer formed by copolymerization of a modified acrylic monomer and acrylonitrile, and a copolymer formed by copolymerization of a modified acrylic monomer and acrylamide.

[0051] It can be understood that the polymer of acrylic monomers has an adhesive effect, which can achieve the bonding of the composite coating and the base film, and is not easy to separate. The present application adopts at least one of a homopolymer formed by homopolymerization of modified acrylic monomers, a copolymer formed by copolymerization of multiple modified acrylic monomers, a copolymer formed by copolymerization of modified acrylic monomers and acrylonitrile, and a copolymer formed by copolymerization of modified acrylic monomers and acrylamide. The polymer of modified acrylic monomers has the characteristics of adhesion, dispersibility, wettability, etc., which can reduce the introduction of additives when preparing the slurry, reduce the risk of isolation short circuit, thereby reducing the short circuit rate of the battery, and also shorten the preparation time of the slurry.

[0052] In some embodiments, the base film has a first thickness H1, and the composite coating has a second thickness H2, satisfying: 1.25≤H1 / H2≤20. Specifically, the ratio of the first thickness H1 to the second thickness H2 can be any one of 1.25, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, or a range consisting of any two values.

[0053] It can be understood that by making the ratio of the first thickness H1 to the second thickness H2 satisfy: 1.25≤H1 / H2≤20, the risk of isolation short circuit can be reduced while ensuring good ionic conductivity, thereby reducing the short circuit rate of the battery.

[0054] In some embodiments, the base film has a first thickness H1, which satisfies: 5 μm ≤ H1 ≤ 20 μm. Specifically, the value of the first thickness H1 (unit: μm) can be any one of 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 or a range consisting of any two values.

[0055] It can be understood that when the thickness of the base film is too large, it will affect the ionic conductivity of the prepared diaphragm. When the thickness of the base film is too small, it will affect the puncture resistance of the prepared diaphragm. The present application makes the thickness of the base film satisfy: 5μm≤H1≤20μm, so that the diaphragm can have good ionic conductivity and good puncture resistance.

[0056] In some embodiments, the composite coating has a second thickness H2, which satisfies: 1 μm≤H2≤4 μm. Specifically, the value of the second thickness H2 (unit: μm) can be any one of 1, 2, 3, 4, or a range consisting of any two values.

[0057] It can be understood that when the thickness of the composite coating is too large, it will affect the ionic conductivity of the prepared membrane, and the composite coating will also easily fall off. When the thickness of the composite coating is too small, it will affect the heat resistance and wettability of the prepared membrane. The present application controls the thickness of the composite coating to meet the conditions of 1μm≤H2≤4μm, so that the membrane can have good ionic conductivity while having good heat resistance and wettability.

[0058] In some embodiments, the base film is selected from polyethylene (PE) or polypropylene (PP).

[0059] A second aspect of the present application provides a method for preparing a diaphragm, comprising:

[0060] Mixing the composite binder and the solvent for the first time to obtain a first mixture;

[0061] Mixing the coating main material and the first mixture for a second time to obtain a coating slurry;

[0062] Applying the coating slurry on at least one side of the base film to obtain a diaphragm;

[0063] The composite binder is selected from polymers of modified acrylic monomers;

[0064] The modified acrylic monomer includes an acrylic monomer having a side chain;

[0065] The side chain includes a first branch chain, and the first branch chain is selected from at least one of carboxymethyl, hydroxyethyl and hydroxypropyl.

[0066] It can be understood that the present application provides a composite adhesive, which is selected from a polymer of modified acrylic monomers. By modifying the acrylic monomers, side chains are formed on the acrylic monomers, and the side chains include a first branch chain, which is selected from at least one of carboxymethyl, hydroxyethyl, and hydroxypropyl. The hydrogen bonds in the first branch chain can associate with water molecules in the slurry, increase the fluid volume of the polymer itself, and reduce the free activity space of the coating main material in the coating slurry, so that the coating slurry can achieve an anti-settling effect. At the same time, the branch chain is easy to ionize positively charged hydrogen ions, and the coating slurry prepared under the repulsion of like charges has good dispersibility; the composite adhesive and the solvent are mixed for the first time to obtain a first mixture; and the coating main material is mixed with the first mixture for the second time to obtain a coating slurry. Since the polymer of the modified acrylic monomer has the characteristics of adhesion, dispersibility, wettability, etc., compared with the preparation of conventional slurries, the introduction of additives such as dispersants and wetting agents is reduced, and the preparation time of the slurry is also shortened, thereby reducing the production cost.

[0067] In some embodiments, the side chain further includes a second branch chain, and the second branch chain is selected from at least one of a hyperbranched polyether, a polyether-modified siloxane, a polyether-modified acetylenic glycol, and a polyether-modified olefinic glycol.

[0068] In some embodiments, the coating slurry may be coated on at least one side of the base film by gravure roll coating or rotor rotary spray coating.

[0069] In some embodiments, acrylic monomers react with cellulose and carboxyl groups through thermal reactions to form carboxymethyl branches on the main chain of acrylic monomers. During the reaction, the temperature is 40-90° C., the pressure is 0.1-2 MPa, the reaction time is 3-24 hours, and the initiator is selected from at least one of ammonium persulfate, potassium persulfate, and sodium persulfate.

[0070] In some embodiments, acrylic monomers react with cellulose and hydroxyl groups through thermal reaction to form hydroxyethyl or hydroxypropyl side chains on the main chain of the acrylic monomers. During the reaction, the temperature is 40-90° C., the pressure is 0.1-2 MPa, the reaction time is 3-24 hours, and the initiator is selected from at least one of ammonium persulfate, potassium persulfate, and sodium persulfate.

[0071] In some embodiments, acrylic monomers and hyperbranched polyethers are reacted thermally to form hyperbranched polyether branches on the main chain of the acrylic monomer. During the reaction, the temperature is 35 to 95° C., the pressure is 0.1 to 2 MPa, the reaction time is 3 to 24 hours, and the initiator is selected from at least one of ammonium persulfate, potassium persulfate, and sodium persulfate.

[0072] In some embodiments, acrylic monomers and polyether-modified siloxanes are thermally reacted to form polyether-modified siloxane side chains on the main chain of the acrylic monomers. During the reaction, the temperature is 35 to 95° C., the pressure is 0.1 to 2 MPa, the reaction time is 3 to 24 hours, and the initiator is selected from at least one of ammonium persulfate, potassium persulfate, and sodium persulfate.

[0073] In some embodiments, acrylic monomers and polyether-modified acetylene glycols are subjected to a thermal reaction to form polyether-modified acetylene glycol side chains on the main chain of the acrylic monomers. During the reaction, the temperature is 35 to 95° C., the pressure is 0.1 to 2 MPa, the reaction time is 3 to 24 hours, and the initiator is selected from at least one of ammonium persulfate, potassium persulfate, and sodium persulfate.

[0074] In some embodiments, acrylic monomers and polyether-modified ethylene glycols are subjected to a thermal reaction to form polyether-modified ethylene glycol side chains on the main chain of the acrylic monomers. During the reaction, the temperature is 35 to 95° C., the pressure is 0.1 to 2 MPa, the reaction time is 3 to 24 hours, and the initiator is selected from at least one of ammonium persulfate, potassium persulfate, and sodium persulfate.

[0075] In some embodiments, the polymer of the modified acrylic monomer is selected from at least one of a homopolymer formed by homopolymerization of a modified acrylic monomer, a copolymer formed by copolymerization of multiple modified acrylic monomers, a copolymer formed by copolymerization of a modified acrylic monomer and acrylonitrile, and a copolymer formed by copolymerization of a modified acrylic monomer and acrylamide.

[0076] In some embodiments, the mass ratio of the coating main material, the composite binder and the solvent is 93-97:3-7:95-99. Specifically, the mass ratio of the coating main material, the composite binder and the solvent can be any one of 93:7:95, 94:6:96, 95:5:97, 97:3:98, 95:5:99 or a range between any two ratios.

[0077] It can be understood that the solvent is used to dissolve the composite adhesive and the coating main material to form a coating slurry. The coating main material is used to improve the heat resistance and wettability of the base film. The composite adhesive is mainly used to make the composite coating formed by the coating slurry adhere to the base film and not easy to fall off. At the same time, it also has the function of dispersing the coating main material in the solvent. The present application can form a coating slurry with good dispersion and wettability by controlling the mass ratio of the coating main material, the composite adhesive and the solvent to 93~97:3~7:95~99.

[0078] In some embodiments, the solvent is selected from at least one of deionized water and ultrapure water.

[0079] In some embodiments, the first mixing time is 20 to 40 minutes. Specifically, the first mixing time (unit: min) can be any one of 20, 25, 30, 35, 40 or a range consisting of any two values.

[0080] It can be understood that the present application provides a composite adhesive, which includes a polymer of a modified acrylic monomer. The acrylic monomer is modified to form a side chain on the acrylic monomer, and the side chain includes a first branch chain. The first branch chain is selected from at least one of carboxymethyl, hydroxyethyl, and hydroxypropyl. The first branch chain contains a hydrogen bond and has good compatibility with the solvent. Therefore, when the mixing time of the composite adhesive and the solvent meets 20 to 40 minutes, a uniformly mixed first mixed liquid can be obtained, which shortens the preparation time compared to conventional slurry preparation.

[0081] In some embodiments, the second mixing time is 100 to 180 minutes. Specifically, the second mixing time (unit: min) can be any one of 100, 110, 120, 130, 140, 150, 160, 170, 180 or a range consisting of any two values.

[0082] It is understandable that the present application provides a composite adhesive, the composite adhesive is selected from a polymer of modified acrylic monomers, and a side chain is formed on the acrylic monomer by modifying the acrylic monomer, the side chain includes a first branch chain, the first branch chain is selected from at least one of carboxymethyl, hydroxyethyl, and hydroxypropyl, and the first branch chain contains hydrogen bonds, which has good compatibility with the solvent. At the same time, the hydrogen bonds in the first branch chain can associate with water molecules in the slurry, increase the fluid volume of the polymer itself, and reduce the free activity space of the coating main material in the coating slurry, so that the coating slurry can achieve an anti-settling effect, and at the same time, the branch chain ionizes positively charged hydrogen ions to achieve a dispersion effect. Therefore, when the mixing time of the first mixed liquid and the coating main material meets 100 to 180 minutes, a uniformly mixed coating slurry can be obtained, which shortens the preparation time compared to conventional slurry preparation.

[0083] A third aspect of the present application provides a battery, comprising the diaphragm as described above or a diaphragm prepared by the diaphragm preparation method as described above.

[0084] It can be understood that the use of the diaphragm provided in the present application or the diaphragm prepared by the preparation method of the diaphragm provided in the present application can reduce the risk of isolation short circuit, thereby reducing the short circuit rate of the battery.

[0085] A fourth aspect of the present application provides an electrical device, comprising the battery as described above.

[0086] It is understandable that electrical equipment includes, but is not limited to, backup power supplies, motors, electric vehicles, electric motorcycles, power-assisted bicycles, bicycles, power tools, large household batteries, etc.

[0087] The present application is described below in conjunction with specific embodiments.

[0088] Example 1

[0089] The base film material is selected from PE, and the base film has a first thickness H1, and the first thickness H1 is 9 μm;

[0090] Weigh 95g of the coating main material, 5g of the composite binder and 97g of deionized water for later use;

[0091] The coating main material includes 83.6g of aluminum oxide and 11.4g of polymethyl methacrylate, and the particle size of the coating main material is 0.3-6.0μm;

[0092] At room temperature and pressure, the composite binder and deionized water are mixed for the first time to obtain a first mixture; the first mixing time is 30 minutes;

[0093] At room temperature and pressure, the coating main material is mixed with the first mixture for a second time to obtain a coating slurry; the second mixing time is 150 minutes;

[0094] The coating slurry is coated on both sides of the base film by gravure roller coating to form a composite coating, and a diaphragm is obtained after heat treatment, wherein the composite coating has a second thickness H2, and the second thickness H2 is 2 μm;

[0095] The composite adhesive is a homopolymer formed by homopolymerization of modified acrylic monomers; the modified acrylic monomers are acrylic monomers with a first branch chain and a second branch chain, the first branch chain is a carboxymethyl group, and the second branch chain is a hyperbranched polyether.

[0096] Example 2

[0097] The preparation method of Example 2 is the same as that of Example 1, except that the composite adhesive is a homopolymer formed by homopolymerization of a modified acrylic monomer; the modified acrylic monomer is an acrylic monomer having a side chain, the side chain includes a first branch chain, and the first branch chain is a carboxymethyl group.

[0098] Example 3

[0099] The preparation method of Example 3 is the same as that of Example 1, except that the composite adhesive is a copolymer formed by copolymerizing a first modified acrylic monomer and a second modified acrylic monomer; the first modified acrylic monomer is an acrylic monomer having a first branch, the first branch is a carboxymethyl group, and the second modified acrylic monomer is an acrylic monomer having a first branch and a second branch, the first branch is a carboxymethyl group, and the second branch is a hyperbranched polyether.

[0100] Example 4

[0101] The preparation method of Example 4 is the same as that of Example 1, except that the coating slurry is coated on one side of the base film by gravure roller coating to form a composite coating.

[0102] Embodiment 5-6

[0103] The preparation methods of Examples 5 to 6 are the same as those of Example 1, except that the thickness of the composite coating is adjusted.

[0104] Embodiments 7 to 9

[0105] The preparation methods of Examples 7 to 9 are the same as those of Example 1, except that the thickness of the base film is adjusted.

[0106] Embodiments 10 to 12

[0107] The preparation methods of Examples 10 to 12 are the same as those of Example 4, except that the thickness of the base film is adjusted.

[0108] Comparative Example 1

[0109] The preparation method of Comparative Example 1 is the same as that of Example 1, except that the composition and preparation method of the coating slurry are different:

[0110] Weigh 95g of the coating material, 3g of the adhesive, 2g of the additive, and 97g of deionized water for later use;

[0111] The coating main material includes 83.6g of aluminum oxide and 11.4g of polymethyl methacrylate, and the particle size of the coating main material is 0.3-6.0μm;

[0112] The adhesive is selected from 3g polyacrylates;

[0113] The additives included 1.4 g of sodium carboxymethyl cellulose (anti-settling agent), 0.5 g of ammonium salt (dispersant) and 0.1 g of acetylene glycol (surfactant).

[0114] Preparation method of coating slurry

[0115] First, add 0.5g of ammonium salt dispersant into 97g of deionized water and stir for 30min, then add 83.6g of aluminum oxide and 11.4g of polymethyl methacrylate and stir for 60min, then add 1.4g of sodium carboxymethyl cellulose aqueous solution and stir for 100min, then add 3g of polyacrylate adhesive and stir for 60min, and finally add 0.1g of enediol and stir for 30min to obtain a coating slurry.

[0116] Comparative Example 2

[0117] The preparation method of Comparative Example 2 is the same as that of Comparative Example 1, except that the coating slurry is coated on one side of the base film by gravure roller coating to form a composite coating.

[0118] Comparative Examples 3 to 5

[0119] The preparation methods of Comparative Examples 3 to 5 are the same as those of Comparative Example 1, except that the thickness of the base film is adjusted.

[0120] Comparative Examples 6 to 8

[0121] The preparation methods of Comparative Examples 6 to 8 are the same as those of Comparative Example 2, except that the thickness of the base film is adjusted.

[0122] Comparative Examples 9 to 11

[0123] The preparation methods of Comparative Examples 9 to 11 are the same as those of Example 1, except that the thickness of the composite coating is adjusted.

[0124] The following uses lithium batteries as an example to explain battery assembly.

[0125] (1) Preparation of positive electrode sheets: Lithium iron phosphate or ternary nickel cobalt manganese materials are used to prepare slurry, which is coated on carbon-coated aluminum foil and treated to obtain positive electrode sheets. The lithium iron phosphate or ternary nickel cobalt manganese in the coating accounts for 96.5%, and the rest is adhesive, conductive agent, etc.

[0126] (2) Preparation of negative electrode sheet: Artificial graphite is used to prepare slurry, and the slurry is coated on copper foil and processed to obtain negative electrode sheet. The artificial graphite in the coating accounts for 95.5%, and the rest is adhesive, conductive agent, etc.

[0127] (3) Preparation of electrode group: The composite separator and the negative electrode plate are bonded by hot roller hot pressing using a thermal composite process, and the hot roller temperature is 70 to 100°C; the unit formed after hot pressing is cut into single pieces by a hot cutter to form a sandwich structure of separator-negative electrode-separator; the sandwich structure and the positive electrode plate are stacked into an electrode group in the form of a stack, and hot pressed at 85 to 95°C using a flat hot press to complete the preparation of the electrode group.

[0128] (4) Packaging and injection: The prepared electrode group is packaged in a square shell form and then injected with electrolyte.

[0129] (5) Pre-charging and formation: Pre-charging and formation of the battery cells to complete the preparation of the battery.

[0130] Test method:

[0131] (1) Thickness test method: Use a Mahr thickness gauge or a micrometer to test the thickness.

[0132] (2) Battery Hi-pot resistance short-circuit rate test method: voltage 250V, time 2s.

[0133] Table 1 shows the parameter settings and test results of Examples 1 to 14 and Comparative Examples 1 to 11

[0134]

[0135]

[0136] Result analysis:

[0137] It can be seen from the test results of Examples 1 to 12, Comparative Examples 1 to 11 and Table 1 that the diaphragm prepared by using the composite adhesive provided by the present application can reduce the risk of isolation short circuit, thereby reducing the short circuit rate of the battery.

[0138] It can be seen from the test results of Example 1, Example 4, Comparative Examples 1 to 2 and Table 1 that the diaphragm prepared using the composite adhesive provided by the present application can reduce the short-circuit rate of the battery; when the base film thickness is 9 μm and the composite coating thickness is 2 μm, a composite coating is formed on both sides of the base film, which can further reduce the short-circuit rate of the battery.

[0139] It can be seen from the test results of Example 1, Examples 7 to 9, Comparative Examples 3 to 5 and Table 1 that the diaphragm prepared using the composite adhesive provided by the present application can reduce the short-circuit rate of the battery; when the thickness of the composite coating is the same, the short-circuit rate of the battery is slightly reduced as the thickness of the base film increases.

[0140] It can be seen from the test results of Example 4, Examples 10 to 12, Comparative Examples 6 to 8 and Table 1 that the diaphragm prepared using the composite adhesive provided by the present application can reduce the short-circuit rate of the battery; when the thickness of the composite coating is the same, the short-circuit rate of the battery is slightly reduced as the thickness of the base film increases.

[0141] It can be seen from the test results of Example 1, Examples 5 to 6, Comparative Examples 9 to 11 and Table 1 that the diaphragm prepared using the composite adhesive provided by the present application can reduce the short-circuit rate of the battery; when the thickness of the base film is the same and the thickness of the composite coating increases, the short-circuit rate of the battery is slightly reduced; when the thickness of the base film is the same and the thickness of the composite coating decreases, the short-circuit rate of the battery is slightly increased.

[0142] In summary, although the embodiments of the present application are described in detail above, the above embodiments are not intended to limit the present application, and ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein; and these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A diaphragm, characterized in that: It comprises a base film and a composite coating disposed on at least one side of the base film, wherein the composite coating comprises a coating main material and a composite adhesive; the composite adhesive is selected from a polymer of modified acrylic monomers; The modified acrylic monomer includes an acrylic monomer having a side chain; The side chain includes a first branch chain, and the first branch chain is selected from at least one of carboxymethyl, hydroxyethyl, and hydroxypropyl.

2. The diaphragm according to claim 1, characterized in that The side chain further includes a second branch chain, and the second branch chain is selected from at least one of hyperbranched polyether, polyether-modified siloxane, polyether-modified acetylene glycol, and polyether-modified olefin glycol.

3. The diaphragm according to claim 1, characterized in that The mass ratio of the coating main material to the composite adhesive is 93-97:3-7.

4. The diaphragm according to claim 1, characterized in that The acrylic monomer is selected from at least one of acrylic acid and methacrylic acid; and / or, The coating main material is selected from at least one of inorganic oxides, polymethyl methacrylate, polyethylene spheres, and polytetrafluoroethylene; and / or, The polymer of the modified acrylic monomer is at least one selected from a homopolymer formed by homopolymerization of a modified acrylic monomer, a copolymer formed by copolymerization of multiple modified acrylic monomers, a copolymer formed by copolymerization of a modified acrylic monomer and acrylonitrile, and a copolymer formed by copolymerization of a modified acrylic monomer and acrylamide.

5. The diaphragm according to claim 1, characterized in that The base film has a first thickness H1, and the composite coating has a second thickness H2, satisfying: 1.25≤H1 / H2≤20; and / or, The base film has a first thickness H1, which satisfies: 5 μm≤H1≤20 μm; and / or, The composite coating has a second thickness H2, which satisfies: 1 μm≤H2≤4 μm.

6. A method for preparing a diaphragm, characterized in that: include: Mixing the composite binder and the solvent for the first time to obtain a first mixture; Mixing the coating main material with the first mixture for a second time to obtain a coating slurry; Applying the coating slurry on at least one side of the base film to obtain a diaphragm; The composite binder is selected from polymers of modified acrylic monomers; The modified acrylic monomer includes an acrylic monomer having a side chain; The side chain includes a first branch chain, and the first branch chain is selected from at least one of carboxymethyl, hydroxyethyl, and hydroxypropyl.

7. The method for preparing a diaphragm according to claim 6, characterized in that: The side chain further includes a second branch chain, and the second branch chain is selected from at least one of a hyperbranched polyether, a polyether-modified siloxane, a polyether-modified acetylenic glycol, and a polyether-modified olefinic glycol; and / or, The polymer of the modified acrylic monomer is at least one selected from a homopolymer formed by homopolymerization of a modified acrylic monomer, a copolymer formed by copolymerization of multiple modified acrylic monomers, a copolymer formed by copolymerization of a modified acrylic monomer and acrylonitrile, and a copolymer formed by copolymerization of a modified acrylic monomer and acrylamide.

8. The method for preparing a diaphragm according to claim 6, characterized in that: The mass ratio of the coating main material, the composite binder and the solvent is 93-97:3-7:95-99; and / or, The first mixing time is 20 to 40 minutes; and / or, The second mixing time is 100 to 180 minutes.

9. A battery, characterized in that: The invention comprises a diaphragm as claimed in any one of claims 1 to 5 or a diaphragm prepared by the diaphragm preparation method as claimed in any one of claims 6 to 8.

10. An electrical device, characterized in that: Comprising the battery as claimed in claim 9.