Transparent high-strength all-polyimide nano-composite film and preparation method thereof
By preparing a transparent and high-strength all-polyimide nanocomposite film and using coaxial electrospinning and selective dissolution technology, the problems of low mechanical properties of polyimide materials and difficulty in uniform dispersion of nanofillers are solved, achieving high transparency and Excellent mechanical properties.
Patent Information
- Application Number
- CN202410978682.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Existing polyimide materials have low mechanical properties and are difficult to meet the needs in certain applications. Moreover, there are problems of uniform dispersion and high cost when adding nanofillers to the matrix.
By preparing a transparent high-strength all-polyimide nanocomposite film, coaxial electrospinning technology is used to generate a core-shell nanofiber film, and the uniform dispersion and high strength of the nanofibers are achieved through selective dissolution and hot pressing methods, and the polymerization is controlled. The volume ratio of imide and polyamic acid can be adjusted to adjust the hole content.
It achieves high transparency, excellent tensile strength and Young's modulus, overcomes the structural defects and interface compatibility problems of traditional nanofiber membranes, and is suitable for mass production.
Smart Images

Figure CN118756428A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials with high mechanical properties, and in particular to a transparent high-strength all-polyimide nanocomposite film and a preparation method thereof. Background Art
[0002] Nowadays, polymer-based composites, as advanced functional materials, have attracted more and more attention from researchers due to their relatively excellent combination properties with organic components, such as flexibility, low dielectric properties, high breakdown strength, durability and super thermal stability. Among them, polyimide (PI), as a typical engineering polymer material, has been widely used as insulation materials, microelectronics, and even aerospace and aircraft parts in the past few years due to its excellent electrical insulation, thermal properties and chemical resistance. However, the relatively low mechanical properties of pure PI limit its demand in some special applications.
[0003] In order to improve the mechanical properties of PI, an effective method is to add nanofillers such as hyperbranched polysiloxane (NH2-HBPSi), carbon nanotubes (CNTs), graphene oxide (GO), and graphene nanoribbons (GNRs) through strong interfacial interactions. However, it is currently impossible to add a large amount of nanofillers to the PI matrix, and there are also problems such as difficulty in uniform dispersion and high cost. Most research is still difficult to industrialize on a large scale. In addition, another effective strategy is to modify the structure by introducing heterocycles and hydrogen bonds to increase the intermolecular force, but this method has a complex synthesis route, high cost, and low yield. Summary of the invention
[0004] The purpose of the present invention is to address the defects of the prior art and provide a transparent, high-strength all-polyimide nanocomposite film and a preparation method. The material has a large number of nano-scale pores inside, and by controlling the volume ratio of polyimide and polyamic acid, a more controllable content of the pores can be achieved, so that the film has an extremely low dielectric constant and maintains high transparency.
[0005] The present invention provides a method for preparing a transparent high-strength all-polyimide nanocomposite film, comprising:
[0006] Step 1: dissolving a soluble polyimide in a polar organic solvent to obtain a polyimide solution;
[0007] Step 2: Add aromatic diamine to a polar organic solvent, and then add aromatic dianhydride after the aromatic diamine is dissolved to react to obtain a polyamic acid solution. Preferably, the reaction process is carried out under an inert atmosphere and an ice bath, the reaction temperature is 0 to 5° C., and the reaction time is 6 to 12 hours.
[0008] Step 3: Use the polyimide solution as the outer diameter fluid and the polyamic acid solution as the inner diameter fluid for coaxial electrospinning. A core-shell nanofiber membrane with no beads, smooth fiber surface and uniform fiber diameter is obtained, the outer shell is polyimide and the core material is polyamic acid. Then heat the film to thermally imidize the polyamic acid to obtain a core-shell polyimide nanofiber membrane. The thermal imidization process includes the first stage, the second stage, the third stage, the fourth stage and the fifth stage: the temperature of the first stage is 80-110°C, the temperature of the second stage is 110-130°C, the temperature of the third stage is 150-180°C, the temperature of the fourth stage is 210-240°C, and the temperature of the fifth stage is 290-320°C. The insulation time of each stage is 30-120min independently.
[0009] Step 4: Soak the core-shell polyimide nanofiber membrane in a mixed organic solvent. The mixed organic solvent is used to adjust the solubility and selectively dissolve the outer shell of the core-shell polyimide nanofiber membrane with a large specific surface area in a confined space.
[0010] Step 5: hot-press the soaked core-shell polyimide film and wash it to obtain a full polyimide nanofiber composite membrane. During the hot-pressing process, the dissolved portion of the outer layer serves as the filling phase, and the undissolved portion of the inner layer serves as the supporting phase. Preferably, the hot-pressing temperature is 60 to 180°C, the pressure is 0 to 4MPa, and the hot-pressing time is 10 to 60min. Preferably, the washing process adopts an immersion method, the immersion solution is one or more of water and ethanol, and the immersion time is 12 to 48h.
[0011] Further, in step 1, the polar organic solvent includes one or more of dichloromethane, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, ethanol, acetone, toluene, amyl acetate, dimethyl sulfoxide, and chloroform, and the mass fraction of the soluble polyimide solution is 10 to 30 wt %. Preferably, the organic solvent is N,N-dimethylacetamide.
[0012] Furthermore, in step 2, the aromatic diamine includes 4,4'-diaminodiphenyl ether.
[0013] Furthermore, in step 2, the aromatic dianhydride includes bisphenol A diether dianhydride.
[0014] Furthermore, in step 3, the inner and outer diameter flow rate ratio of the electrospinning is 1:1 to 1:10, the needle specification is 15-26, the liquid flow rate is 0.1-3mL / h, the receiving distance is 10-15cm, the voltage is 10-25Kv, the drum speed is 100-600rpm, and the spinning time is 1-8h.
[0015] Further, in step 2, the molar ratio of the aromatic diamine to the aromatic dianhydride is 1:1.02. Preferably, the molar ratio of the aromatic diamine to the aromatic dianhydride is 1:1.
[0016] Further, in step 2, the polar organic solvent includes one or more of dichloromethane, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, ethanol, acetone, toluene, amyl acetate, dimethyl sulfoxide, and chloroform, and the mass fraction of the polyamic acid solution is 5 to 30 wt %. Preferably, the mass fraction of the polyamic acid solution is 12 wt %.
[0017] Furthermore, in step 3, the volume ratio of the polyimide and the polyamic acid is 1:4-1:2. Furthermore, in the coaxial electrospinning process, the inner and outer diameter flow rate ratio is 1:1 to 1:10, the needle specification is 15 to 26, the liquid flow rate is 0.2 to 3 mL / h, the receiving distance is 10 to 15 cm, the voltage is 10 to 25 Kv, and the drum speed is 100 to 600 rpm.
[0018] Further, in step 4, the mixed organic solvent includes a plurality of dichloromethane, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, ethanol, acetone, toluene, amyl acetate, dimethyl sulfoxide, chloroform and water, the solvent solubility is 0 to 50wt%, and the soaking time is 0 to 10min. . Preferably, it is a 5wt% ethanol N,N-dimethylacetamide solution. Further, in step 4, the mixed organic solvent is a mixed solvent of DMAc and ethanol, wherein the mass percentage of DMAc is 2 to 50wt%, preferably 5wt%.
[0019] A transparent high-strength all-polyimide nanocomposite film is obtained by using any of the above preparation methods.
[0020] The beneficial effects of the present invention are:
[0021] 1. The present invention selectively dissolves nanofibers with a core-shell structure with a large specific surface area in a confined space, realizes the self-"fusion" lap of nanofibers and the self-reinforcement of long fibers, and successfully prepares a composite film that is transparent, high-strength, high-modulus, and high-nano filling. Compared with the traditional addition of nanomaterials, the composite film prepared by this method does not need to consider the problems of low addition, agglomeration, and uneven dispersion. The content of nanomaterials can be added according to the ideal content and can be evenly dispersed, while solving the problem of interface compatibility. Compared with traditional electrospun nanofibers, this composite film overcomes the problems of opacity and structural defects, has high light transmittance (higher than 85%), and has excellent tensile strength (323.28MPa) and Young's modulus (9.50±0.90GPa).
[0022] 2. The composite film prepared by the present invention makes up for the structural defects of the electrospun fiber membrane. The external dissolved fibers "fuse" and bond to the internal fibers, maintaining the orientation of the internal fibers. The good compatibility between the highly oriented polymer fibers and the matrix enables them to play a role in stress transfer and bridging during stretching or stress, thereby significantly improving the mechanical properties of the material.
[0023] 3. In the preparation method of the present invention, since the outer shell is soluble and the core material is insoluble when preparing the core-shell polyimide nanofiber membrane, the solubility range can be controlled during preparation, the preparation consistency is high, and nanomaterials can be directly added by coaxial electrospinning without complicated additional processing techniques. The operation is simple, and controllable addition of nanomaterials can be achieved, which is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 are photographs of PI-4-1 in Example 1, PI-2-1 in Example 2, PI-1 in Comparative Example 1, and PI-2 in Comparative Example 2;
[0025] Figure 2 is a scanning electron microscope photograph of PI-4-1 in Example 1;
[0026] Figure 3 is a scanning electron microscope photograph of PI-2-1 in Example 2;
[0027] Figure 4 is a scanning electron microscope photo of PI-1 in Comparative Example 1;
[0028] Figure 5 is a scanning electron microscope photo of PI-2 in Comparative Example 2;
[0029] Figure 6 is a spectrum of the transmittance of PI-4-1 in Example 1, PI-2-1 in Example 2, PI-1 in Comparative Example 1, and PI-2 in Comparative Example 2;
[0030] Figure 7 are stress-strain spectra of PI-1 in comparative example 1, PI-2 in comparative example 2, PI-4-1 in example 1, and PI-2-1 in example 2;
[0031] Figure 8 is the tensile strength spectrum of PI-1 in Comparative Example 1, PI-2 in Comparative Example 2, PI-4-1 in Example 1, and PI-2-1 in Example 2;
[0032] Fig. 9 It is the Young's modulus spectrum of PI-1 in Comparative Example 1, PI-2 in Comparative Example 2, PI-4-1 in Example 1, and PI-2-1 in Example 2;
[0033] Fig.10 This is the infrared spectrum of the core material polyimide in Example 1 and Example 2. DETAILED DESCRIPTION
[0034] The present invention is further described below by way of examples and comparative examples. The drugs used in the following examples are all commercially available products unless otherwise specified, and the methods used are all conventional methods in the art unless otherwise specified.
[0035] Example 1
[0036] A method for preparing a transparent high-strength all-polyimide nanocomposite film comprises the following steps:
[0037] (1) Preparation of polyimide solution
[0038] Weigh 4.05 g of soluble polyimide powder (molecular weight 2-10w), add 11.95 g of N,N-dimethylacetamide, stir until it is completely dissolved, and continue to stir at room temperature for 12 hours to obtain a polyimide solution.
[0039] (2) Preparation of polyamic acid solution
[0040] Under ice bath and nitrogen conditions, 5 mmol of 4,4'-diaminodiphenyl ether was added to a three-necked flask, and then N,N-dimethylacetamide was added. After the diamine monomer was completely dissolved, 5 mmol of bisphenol A diether dianhydride was added, stirred to dissolve, and then stirred and reacted at low temperature for 6 hours to obtain a 12 wt% polyamic acid solution.
[0041] (3) Preparation of core-shell polyimide nanofiber films
[0042] The polyimide solution was poured into a 20 mL syringe for the outer diameter spinning solution. The electrospinning process parameters used were: voltage 14 KV, push speed 0.20 mL / h, needle size 17, receiving distance 12 cm, and drum speed 200 rpm; the polyamic acid solution was poured into a 20 mL syringe for the inner diameter spinning solution. The electrospinning process parameters used were: voltage 14 KV, push speed 0.80 mL / h, needle size 23, and receiving distance The diameter of the roller is 11 cm and the speed of the drum is 200 rpm. The fiber filaments sprayed out of the needle are collected on aluminum foil to obtain a core-shell nanofiber membrane. The outer shell is polyimide and the core material is polyamic acid. The volume ratio of polyimide to polyamic acid is 1:4. The core-shell nanofiber membrane is subjected to programmed thermal imidization. The thermal imidization process is: 80°C for 1h, 120°C for 1h, 180°C for 1h, 240°C for 2h, and 300°C for 1h to obtain a core-shell polyimide nanofiber membrane.
[0043] (4) Selective dissolution of core-shell polyimide nanofiber membranes
[0044] The core-shell polyimide nanofiber membrane was immersed in a mixed solvent of DMAc and C2H5OH, wherein the mass percentage of DMAc was 5wt% and the immersion time was 40s. The immersed core-shell polyimide nanofiber membrane was placed on a polytetrafluoroethylene membrane and the C2H5OH was allowed to volatilize.
[0045] (5) Preparation of all-polyimide nanocomposite membranes
[0046] The volatilized core-shell polyimide nanofiber membrane was placed between two layers of polytetrafluoroethylene membranes, preheated at 130°C for 35 minutes, and then hot-pressed for 10 minutes under a pressure of 1 MPa to obtain a full polyimide nanocomposite membrane.
[0047] (6) Solvent removal from polyimide nanocomposite membrane
[0048] The polyimide nanocomposite film was immersed in 1L of water for 12 hours, and then the immersed polyimide nanocomposite film was placed in an oven and dried at 80°C in a vacuum environment for 8 hours to remove the residual solvent, thereby obtaining a full polyimide nanocomposite film named PI-4-1.
[0049] Example 2
[0050] (1) Preparation of polyimide solution
[0051] Weigh 4.05 g of soluble polyimide powder (molecular weight 2-10w), add 11.95 g of N,N-dimethylacetamide, stir until it is completely dissolved, and continue to stir at room temperature for 12 hours to obtain a polyimide solution.
[0052] (2) Preparation of polyamic acid solution
[0053] Under ice bath and nitrogen atmosphere, 5 mmol 4,4'-diaminodiphenyl ether was added to a three-necked flask, and then N,N-dimethylacetamide was added. After the diamine monomer was completely dissolved, 5 mmol bisphenol A diether dianhydride was added, stirred to dissolve, and then stirred and reacted at low temperature for 6 hours to obtain a 12 wt% polyamic acid solution.
[0054] (3) Preparation of core-shell polyimide nanofiber films
[0055] The polyimide solution was poured into a 20 mL syringe for the outer diameter spinning solution. The electrospinning process parameters used were: voltage of 14 KV, push speed of 0.20 mL / h, needle size of No. 17, receiving distance of 12 cm, and drum speed of 200 rpm; the polyamic acid solution was poured into a 20 mL syringe for the inner diameter spinning solution. The electrospinning process parameters used were: voltage of 14 KV, push speed of 0.40 mL / h, needle size of No. 23, and receiving distance of The diameter of the thin film is 10 cm and the speed of the drum is 200 rpm. The fiber filaments sprayed out of the needle are collected on aluminum foil to obtain a core-shell nanofiber membrane. The outer shell is polyimide and the core material is polyamic acid. The volume ratio of polyimide to polyamic acid is 1:2. The core-shell nanofiber membrane is subjected to programmed thermal imidization. The thermal imidization process is: 80°C for 1h, 120°C for 1h, 180°C for 1h, 240°C for 2h, and 300°C for 1h to obtain a core-shell polyimide nanofiber membrane.
[0056] (4) Selective dissolution of core-shell polyimide nanofiber membranes
[0057] The core-shell polyimide nanofiber membrane was immersed in a mixed solvent of DMAc and C2H5OH, wherein the mass percentage of DMAc was 5wt% and the immersion time was 40s. The immersed core-shell polyimide nanofiber membrane was placed on a polytetrafluoroethylene membrane and the C2H5OH was allowed to volatilize.
[0058] (5) Preparation of all-polyimide nanocomposite membranes
[0059] The volatilized core-shell polyimide nanofiber membrane was placed between two layers of polytetrafluoroethylene membranes, preheated at 130°C for 35 minutes, and then hot-pressed for 10 minutes under a pressure of 1 MPa to obtain a full polyimide nanocomposite membrane.
[0060] (6) Solvent removal from polyimide nanocomposite membrane
[0061] The polyimide nanocomposite film was immersed in 1L of water for 12 hours, and then placed in an oven and dried at 80°C in a vacuum environment for 8 hours to remove the residual solvent, thereby obtaining a full polyimide nanocomposite film named PI-2-1.
[0062] Comparative Example 1
[0063] The polyimide solution prepared in step 1 of Example 1 was vacuum-degassed and cast on a glass substrate by a casting method, and then placed in an oven at 80° C. for 1 h, 120° C. for 1 h, and 180° C. for 1 h to obtain a yellow transparent polyimide film, named PI-1.
[0064] Comparative Example 2
[0065] The polyamic acid solution prepared in step 2 of Example 1 was vacuum-degassed and cast on a glass substrate by a casting method, and then placed in an oven and kept at 80°C for 1 h, 120°C for 1 h, 180°C for 1 h, 240°C for 2 h, and 300°C for 1 h to obtain a colorless and transparent polyimide film, named PI-2.
[0066] Principle description:
[0067] By adjusting the proportion of mixed organic solvents, the outer shell of the core-shell polyimide nanofibers after coaxial electrospinning is selectively dissolved, the dissolved part serves as the filling phase, and the undissolved part of the inner shell serves as the nano-support phase. Through hot pressing, more dissolved fibers fill the gaps inside the membrane, which weakens the light scattering effect inside the membrane and improves the transparency of the film. At the same time, there are a large number of undissolved nanofibers in the film to form a nanofiber skeleton, and the good compatibility between the highly oriented polymer fibers and the matrix enables them to play a role in stress transfer and bridging during stretching or stress, thereby significantly improving the mechanical properties of the material.
[0068] Moreover, the inner shell of the core-shell polyimide nanofiber is insoluble polyimide, and the outer shell is soluble polyimide. When the solvent dissolves, only the outer shell will dissolve. The inner shell fiber is retained as a supporting phase, and the outer shell is used as a filling phase. The filling content can be controlled by the outer diameter flow rate, thereby achieving the purpose of controllable dissolution.
[0069] In the step of "preparation of core-shell polyimide nanofiber film" in Example 1 and Example 2, when the core-shell nanofiber membrane was subjected to program thermal imidization, the core material polyimide was successfully obtained, and the infrared spectrum is shown in FIG. Fig.10 As shown, the chemical reaction equation of the core material polyamic acid is as follows:
[0070]
[0071] Polyimide can be obtained through different synthetic routes, such as one-step or two-step. The polyimide synthesized by the two-step method has lower solubility. Through heat treatment, polyamic acid is completely imidized to form polyimide, which increases the interaction between polyimide molecules and reduces its solubility. Therefore, in the "selective dissolution of core-shell polyimide nanofiber membrane", only the soluble polyimide of the shell is dissolved, and the core polyimide is not dissolved.
[0072] Performance Test:
[0073] Figure 1These are photos of PI-4-1 in Example 1, PI-2-1 in Example 2, PI-1 in Comparative Example 1, and PI-2 in Comparative Example 2. It can be seen that the treated polyimide nanocomposite film still maintains a high transparency.
[0074] Figure 2-5 In particular, scanning electron microscope photos of PI-4-1 in Example 1, PI-2-1 in Example 2, PI-1 in Comparative Example 1, and PI-2 in Comparative Example 2 are shown. As shown in the figure, the cross-sections of the PI-1 and PI-2 films have no obvious defects and holes, while the number of holes in the films from PI-2-1 to PI-4-1 gradually increases. This is because as the content of the soluble polyimide in the shell of the core-shell nanofiber membrane gradually decreases, the content of the dissolved fiber decreases, and more and more holes are difficult to be completely filled.
[0075] Figure 6 The transmittance spectra of PI-1 in Comparative Example 1, PI-2 in Comparative Example 2, PI-4-1 in Example 1, and PI-2-1 in Example 2. As shown in the figure, PI-2-1 and PI-4-1 also maintain high transparency (higher than 85%) compared with PI-1 and PI-2. The reason is that when a beam of light irradiates the surface of the film, part of the incident light is reflected into the air, and part of the light entering the interior of the film is scattered due to the different refractive indexes of the nanofibers and the air in the pores, while most of the light can pass through the film, so that the film has a higher transparency.
[0076] Figure 7 It is the stress-strain spectrum of PI-1 in comparative example 1, PI-2 in comparative example 2, PI-4-1 in embodiment 1, and PI-2-1 in embodiment 2. As shown in the figure, the strain of PI-4-1 is 323.28MPa, and the strain of PI-2-1 is 225.11MPa, which are 4.94 times and 3.44 times higher than PI-1, and 2.04 times and 1.42 times higher than PI-2, respectively. This is because the polyimide composite film contains a large amount of undissolved nanofiber fillers, and the fibers form a nano-network structure in the matrix material, which plays a role in stress transmission and bridging during stretching or stressing.
[0077] Figure 8 and Fig. 9It is the tensile strength and Young's modulus spectrum of PI-1 in comparative example 1, PI-2 in comparative example 2, PI-4-1 in embodiment 1, and PI-2-1 in embodiment 2. The Young's modulus of PI-4-1 is 9.50±0.90GPa, and the Young's modulus of PI-2-1 is 5.98±0.59GPa, which are 2.88 times and 1.81 times higher than PI-1, and 4.60 times and 2.97 times higher than PI-2, respectively. This is because the polyimide composite film contains a large amount of undissolved nanofiber fillers that support the material like reinforced cement, and the good compatibility between the highly oriented polymer fibers and the matrix makes it play a role in stress transfer and bridging during stretching or stressing, thereby significantly improving the mechanical properties of the material.
[0078] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.
Claims
1. A method for preparing a transparent high-strength all-polyimide nanocomposite film, It is characterized in that include: Step 1: dissolving a soluble polyimide in a polar organic solvent to obtain a polyimide solution; Step 2: adding an aromatic diamine to a polar organic solvent, and then adding an aromatic dianhydride after the aromatic diamine is dissolved, and reacting to obtain a polyamic acid solution; Step 3: using the polyimide solution as the outer diameter fluid and the polyamic acid solution as the inner diameter fluid, coaxial electrospinning is performed to obtain a core-shell nanofiber membrane with a polyimide shell and a polyamic acid core, and then heating the film to obtain a core-shell polyimide nanofiber membrane; Step 4: soaking the core-shell polyimide nanofiber membrane in a mixed organic solvent; Step 5: hot-pressing the soaked core-shell polyimide film and washing it to obtain a full polyimide nanofiber composite membrane.
2. A method for preparing a transparent high-strength all-polyimide nanocomposite film according to claim 1, Features: In step 1, the polar organic solvent includes one or more of dichloromethane, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, ethanol, acetone, toluene, amyl acetate, dimethyl sulfoxide, and chloroform, and the mass fraction of the soluble polyimide solution is 10 to 30 wt%.
3. A method for preparing a transparent high-strength all-polyimide nanocomposite film according to claim 1, Features: In step 2, the aromatic diamine is 4,4'-diaminodiphenyl ether, and the aromatic dianhydride is bisphenol A diether dianhydride.
4. The method for preparing a transparent high-strength all-polyimide nanocomposite film according to claim 1, Features: In step 3, the inner and outer diameter flow rate ratio of the electrospinning is 1:1 to 1:10, the needle specification is 15-26, the liquid flow rate is 0.1-3mL / h, the receiving distance is 10-15cm, the voltage is 10-25Kv, the drum speed is 100-600rpm, and the spinning time is 1-8h.
5. The method for preparing a transparent high-strength all-polyimide nanocomposite film according to claim 1, Features: In step 2, the molar ratio of the aromatic diamine to the aromatic dianhydride is 1:1 to 1:1.
02.
6. The method for preparing a transparent high-strength all-polyimide nanocomposite film according to claim 1, Features: In step 2, the polar organic solvent includes one or more of dichloromethane, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, ethanol, acetone, toluene, amyl acetate, dimethyl sulfoxide, and chloroform, and the mass fraction of the polyamic acid solution is 5 to 30 wt%.
7. The method for preparing a transparent high-strength all-polyimide nanocomposite film according to claim 1, Features: In step 3, the volume ratio of the polyimide to the polyamic acid is 1:4-1:
2.
8. The method for preparing a transparent high-strength all-polyimide nanocomposite film according to claim 1, Features: In step 4, the mixed organic solvent includes multiple ones of dichloromethane, tetrahydrofuran, N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, ethanol, acetone, toluene, amyl acetate, dimethyl sulfoxide, chloroform and water, the solvent solubility is 0 to 50wt%, and the immersion time is 0 to 10min.
9. The method for preparing a transparent high-strength all-polyimide nanocomposite film according to claim 8, Features: In step 4, the mixed organic solvent is a mixed solvent of DMAc and ethanol, wherein the mass percentage of DMAc is 2 to 50 wt %.
10. A transparent high-strength all-polyimide nanocomposite film, Features: The method is obtained by any one of claims 1 to 9.
Citation Information
Patent Citations
Nanometer fiber film preparation method
CN104988662A
Preparation method of high-transmittance antibacterial polyimide / chitosan composite nanofiber air filtering membrane as well as product and application thereof
CN113731197A
Polyimide paper / nanofiber composite membrane with double-layer filtration gradient as well as preparation method and application of polyimide paper / nanofiber composite membrane
CN116943448A
Highly flexible, transparent, conductive film using metal nanotrough-metal nanotube embedded colorless polyimide and the fabrication of flexible, transparent, conducting electrodes using the same
KR101789935B1
Ultra-high modulus and high-transmittance polyimide thin film, and preparation method and application therefor
US20230303786A1
Cited By
Preparation method of coaxial spinning polyimide nanofiber membrane
CN121556217A
A method for preparing a coaxial spun polyimide nanofiber membrane
CN121556217B