Preparation method of porous carbon material with gradient aperture

Through the preparation of gradient pore size porous carbon materials, combined with the composite of hard carbon, soft carbon, conductive carbon materials and carbon nanotubes, the problems of insufficient conductivity and cycle stability of porous carbon materials are solved, and the performance and electrolysis of lithium battery negative electrodes are improved. Stability of liquid-electrode SEI membranes for lithium batteries and supercapacitors.

CN118771376APending Publication Date: 2024-10-15ZHEJIANG GEYUAN NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202410771079.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing porous carbon materials have insufficient conductivity and cycle stability in lithium battery anode applications, resulting in limitations in lithium battery performance. In particular, the volume expansion of the silicon anode during the charge and discharge process leads to mechanical instability and interface SEI instability, which affects Battery life and safety features.

Method used

Using the preparation method of gradient pore size porous carbon materials, through the composite of hard carbon, soft carbon, micron-level conductive carbon materials and carbon nanotubes, spray granulation technology is used to prepare porous carbon with gradient pore size to improve conductivity and adhesion. And through the use of phenolic resin and fluorine-containing resin, the sphericity and particle size of the material are controlled, and the electrochemical performance of the material is enhanced.

Benefits of technology

It achieves high specific surface area, good conductivity and sphericity, improves the electrode loading capacity and cycle life of the lithium battery negative electrode, enhances the battery's fast charging performance and the stability of the electrolyte-electrode SEI film, and is suitable for lithium batteries and Supercapacitors and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771376A_ABST
    Figure CN118771376A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a porous carbon material with gradient aperture, which comprises the following steps: (S1) dispersing crushed soft carbon and hard carbon in a solvent, and adding phenolic resin and fluorine-containing resin; (S2) adding a micron-sized conductive carbon material and a carbon nanotube material to obtain a turbid liquid; (S3) carrying out spray granulation on the turbid liquid to obtain a secondary particle precursor with D50 of 5-10 microns, and drying for later use; (S4) carrying out phenolic resin curing on the dried secondary particle precursor at 160-200 DEG C in a protective atmosphere, and then heating to 500-600 DEG C for carbonization treatment to obtain composite secondary carbon particles; and (S5) performing pore-forming activation on the composite secondary carbon particles to obtain the porous carbon material with gradient pore diameters. Porous carbon with gradient pore size distribution is prepared through compounding of multiple kinds of carbon, regulation and control of the proportion of hard carbon to soft carbon and compounding of micron-sized and carbon nanotube materials, and the porous carbon has improved electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of porous carbon, and in particular relates to a method for preparing a porous carbon material with gradient pore sizes. Background Art

[0002] During the discharge process of a lithium battery, lithium ions are transferred from the negative electrode to the positive electrode, and the battery performs work externally. Therefore, the reversible reaction ability of lithium ions with the negative electrode material determines the energy storage effect of the lithium-ion battery, and the improvement of the performance of the lithium-ion battery depends to a certain extent on the improvement of the performance of the negative electrode material. At present, the widely used negative electrode material is graphite material, but the capacity of commercial graphite negative electrode is close to its theoretical specific capacity (372mAh / g), which limits its further application. Therefore, it is urgent to develop negative electrode materials with higher specific capacity. The silicon negative electrode has a very high theoretical specific capacity (4200mAh / g) and a low electrochemical lithium insertion potential, and excellent fast charging performance, which is exactly what is urgently needed for the development of a series of new technology fields such as portable electronic products, drones, new energy vehicles and energy storage battery systems.

[0003] Silicon negative electrodes have a huge volume expansion during the charge and discharge process. The large volume expansion of silicon negative electrodes during the cycle process will lead to poor cycle life and irreversible capacity, which seriously hinders its commercial application. The volume expansion effect causes the mechanical stability of nano-silicon particles and electrode plates to deteriorate, the contact between active particles is poor, and the stability of the surface SEI passivation film is reduced, which makes the life and safety performance of lithium batteries face challenges.

[0004] Silicon and carbon have similar chemical properties and are tightly bound together, so carbon is often used as the preferred matrix for composites with silicon. Chemical vapor deposition technology can effectively fill silicon materials into porous carbon materials, making the advantages of silicon and carbon composites complementary and significantly improving volume expansion. Porous carbon materials have good cycle stability and lithium ions have no significant effect on their interlayer spacing. To a certain extent, they can buffer and adapt to the volume expansion of silicon; in the silicon-carbon composite system, silicon particles act as active materials to provide lithium storage capacity; porous carbon can buffer the volume change of the silicon negative electrode during charge and discharge, and prevent silicon-carbon particles from agglomerating during the charge and discharge cycle. Therefore, silicon-carbon composite materials have absorbed the unique advantages of both, showing high mass specific capacity and long cycle life in lithium batteries, replacing graphite as a new generation of lithium-ion battery negative electrode materials.

[0005] The traditional porous carbon preparation technology is to activate hard carbon (coconut shell carbon, phenolic resin carbide) or soft carbon (asphalt, petroleum coke). However, there is still a lot of room for development in the regulation of the physical and chemical properties of porous carbon (such as specific surface area, pore volume, pore size distribution and electronic ion conductivity). The porous carbon prepared by traditional carbon as raw material has irregular shape. When preparing lithium battery negative electrode, it is far less effective than the silicon-carbon negative electrode with high sphericity. It also has many factors such as high internal resistance, poor adhesion, low electronic conductivity and unstable interface SEI.

[0006] One of the existing technical solutions is to add conductive carbon materials, such as graphene, carbon nanotubes, etc., to reduce the internal resistance of the negative electrode and improve the conductivity. This method reduces the content of active substances in the negative electrode, which leads to a decrease in electrode capacity and limited global improvement in conductivity, thereby reducing the stability and effectiveness of the electrolyte-electrode SEI film. How to improve the conductivity and cycle stability of the negative electrode without reducing the content of active substances is still a huge challenge. Therefore, how to improve the electronic and ionic conductivity and interface stability of silicon-carbon negative electrode materials and improve their fast charging and long cycle performance is an important issue facing current technology. Summary of the invention

[0007] In order to solve the problem that the electrochemical performance of porous carbon as a silicon-carbon negative electrode material in the prior art is not good enough and the pore size distribution is not rich enough, the present invention proposes a preparation method of porous carbon material with gradient pore size, which uses the different acceptance of hard carbon and soft carbon for activation to create porous carbon with gradient pore size distribution. Specifically, the present invention provides the following technical solutions to solve the above technical problems:

[0008] A method for preparing a porous carbon material with gradient pore sizes comprises the following steps:

[0009] (S1) crushing soft carbon and hard carbon to disperse in solvent, adding phenolic resin and fluorine-containing resin;

[0010] (S2) adding micron-sized conductive carbon material and carbon nanotube material to obtain a suspension;

[0011] (S3) spraying and granulating the suspension to obtain a secondary particle precursor with a D50 of 5-10 μm, and drying for later use;

[0012] (S4) curing the dried secondary particle precursor with a phenolic resin at 160-200° C. under a protective atmosphere, and then heating it to 500-600° C. for carbonization to obtain composite secondary carbon particles;

[0013] (S5) The composite secondary carbon particles are activated to form pores to obtain a porous carbon material with a gradient pore size.

[0014] The scheme of the present invention is to composite multiple carbon materials including hard carbon, soft carbon, micron-level conductive carbon material and carbon nanotube material, and composite hard carbon and soft carbon by spray granulation. Since the reaction degree of hard carbon and soft carbon to activation is different, porous carbon with gradient pore size distribution is prepared. At the same time, by adding micron-level and nano-level carbon nanotube materials, the conductivity and adhesion of porous carbon materials are improved, and the proportion of active materials can be increased when configuring the negative electrode plate, thereby increasing the electrode loading.

[0015] Furthermore, in step (S1), the hard carbon is selected from at least one of biomass pyrolysis carbon (such as coconut shell charcoal) and polymer pyrolysis carbon (such as phenolic resin carbide, epoxy resin carbide); the soft carbon is selected from at least one of asphalt, petroleum coke, and needle coke; the hard carbon accounts for 30-70wt% of the total mass of hard carbon and soft carbon, preferably 50-70%. The inventors found that by regulating the ratio of hard carbon to soft carbon within the above range, porous carbon with high specific surface area and large pore volume can be formed with hard carbon as the substrate. At the same time, the reaction degree of soft carbon to activation is different from that of hard carbon, and a pore distribution different from that of hard carbon is formed on the basis of pore formation of hard carbon, thereby forming a gradient distribution of pores.

[0016] Furthermore, in step (S1), the solvent is selected from at least one of ethanol, N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), and dimethyl sulfoxide (DMSO), and the amount of solvent added is sufficient to achieve sufficient dissolution.

[0017] Furthermore, in step (S1), the molecular weight of the phenolic resin is 5000-100000, and the fluorine-containing resin is selected from at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and ethylene-tetrafluoroethylene copolymer (ETEE); the amount of phenolic resin added is 10-20% of the total mass of the soft carbon and the hard carbon, and the amount of fluorine-containing resin added is 5-10% of the total mass of the soft carbon and the hard carbon.

[0018] Furthermore, in step (S2), the micron-sized conductive carbon material is selected from at least one of Super P and conductive carbon black, the size of the micron-sized conductive carbon material is 1-3 μm, and the amount of the micron-sized conductive carbon material added is 10-15% of the total mass of hard carbon and soft carbon; the carbon nanotube material is selected from water-soluble single-walled carbon nanotubes, and the amount added is 1-2% of the total mass of hard carbon and soft carbon. The present invention adds micron-sized conductive carbon material and carbon nanotubes at the same time. The addition of micron-sized conductive material forms a good conductive network structure in the structured carbon material, and enhances the electrical conductivity of the material. The addition of carbon nanotubes can effectively improve the bonding strength between particles inside the secondary particles, and at the same time improve the intrinsic thermal conductivity, which effectively promotes the high-temperature balling process of the secondary carbon particles.

[0019] Furthermore, in step (S3), the process parameters of spray granulation are that the pressure is controlled at 0.08-0.1MPa and the feed rate is controlled at 100-300mL / min, so that the D50 of the obtained secondary carbon sphere particles is 5-10μm; high temperature curing is treated at 700-1000℃ for 2-5h under a carbonization inert atmosphere; preferably, the inert atmosphere is at least one of nitrogen, argon and helium.

[0020] Furthermore, in step (S4), the protective atmosphere is at least one of nitrogen, helium and argon; the curing time is 2-4 hours, and the carbonization treatment time is 3-5 hours.

[0021] Furthermore, in step (S5), the pore-forming activation is physical activation or chemical activation. The physical activation uses water vapor or carbon dioxide as an activator and is performed at 900-1000°C. The chemical activation is alkali activation, i.e., activation is performed under KOH and / or NaOH conditions and is performed at 750-900°C.

[0022] Compared with the prior art, the beneficial effects of this technical solution are as follows:

[0023] 1. The present invention uses a composite of multiple carbons to adjust the ratio of hard carbon and soft carbon, compound carbon nanotubes of micron-sized conductive carbon materials, and composite multiple carbons together through spray granulation technology. Due to the different degrees of reaction of hard carbon and soft carbon to activation, porous carbon with gradient pore size distribution is prepared. The multi-gradient distribution pore structure can effectively penetrate silane gas along the gradient in pores with different gradients during CVD vapor deposition, thereby achieving a better effect of depositing silicon.

[0024] 2. The present invention adopts spray granulation technology to prepare secondary carbon particle precursor, the particle size is uniform, and the phenolic resin presents a certain sphericity after polycondensation reaction. At the same time, fluorine element is introduced to achieve uniform coating of fluorine element in porous carbon material, thereby improving product performance.

[0025] 3. The scheme of the present invention can achieve precise control of parameters such as carbon material particle size, sphericity, specific surface area, pore volume, pore size, etc. by regulating the ratio of hard carbon, soft carbon, graphite, carbon nanotubes, the amount of phenolic resin used, the condensation temperature and time, and the activation temperature and time.

[0026] 4. The composite functional porous carbon material prepared by the scheme of the present invention has high specific surface area, good conductivity, high sphericity, and uniform particle size, and is suitable for the fields of lithium battery negative electrode, supercapacitor, catalyst carrier, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the nitrogen adsorption curve of the porous carbon prepared in Example 1.

[0028] Figure 2 This is the pore size distribution diagram of the porous carbon prepared in Example 1.

[0029] Figure 3 This is the high-resolution XPS image of the F element of the porous carbon prepared in Example 1.

[0030] Figure 4 This is the 10MPa-100MPa four-terminal powder resistivity diagram of the porous carbon prepared in Example 1.

[0031] Figure 5 This is a 10MPa-100MPa four-terminal powder resistivity diagram of the porous carbon prepared in Comparative Example 1.

[0032] Figure 6 This is the SEM image of the porous carbon prepared in Example 1.

[0033] Figure 7 This is the SEM image of the porous carbon prepared in Comparative Example 2.

[0034] Figure 8 This is the XRD spectrum of Example 1 after CVD deposition.

[0035] Fig. 9 This is the first cycle charge and discharge curve of the negative electrode material prepared from porous carbon in Example 1. DETAILED DESCRIPTION

[0036] Example 1

[0037] (S1) hard carbon (coconut shell charcoal) and soft carbon (petroleum coke) are respectively placed in a ball mill for 48 hours to obtain powders, which are then sieved to obtain crushed hard carbon and soft carbon with a particle size of 100-1000 nm. The hard carbon and soft carbon are dispersed in an ethanol solvent at a mass ratio of 7:3, and 20 wt% of phenolic resin and 10 wt% of PVDF are added to the total mass of the hard carbon and soft carbon;

[0038] (S2) adding 12.5 wt% of the total mass of hard carbon and soft carbon into a micron-sized conductive carbon material Super P and 1.25 wt% of the total mass of hard carbon and soft carbon into a water-soluble single-walled carbon nanotube (0.4% water-soluble single-walled carbon nanotube from Kelude) to obtain a suspension;

[0039] (S3) spray granulation of the suspension, the pressure is controlled at 0.1 MPa, the feed rate is controlled at 300 mL / min, to obtain a secondary particle precursor with a D50 of 7-10 μm, and dry at 80° C. for 12 h for later use;

[0040] (S4) treating the dried secondary particle precursor at 190° C. for 2 h in an argon atmosphere to solidify the phenolic resin, and then heating to 600° C. for 3 h to perform carbonization treatment to obtain composite secondary carbon particles;

[0041] (S5) Under an argon atmosphere, water vapor is introduced into the composite secondary carbon particles at a rate of 28.3 L of water vapor per 1 kg of the composite secondary carbon particles, and a pore-forming activation reaction is carried out at 900° C. for 8 h to obtain a porous carbon material with a gradient pore size.

[0042] Example 2-3

[0043] The other conditions are the same as those in Example 1, except that in step (S1), the ratios of hard carbon and soft carbon added are different, namely 1:1 and 3:7, respectively.

[0044] Embodiment 4-5

[0045] The other conditions are the same as those in Example 1, except that in step (S1), PVDF is replaced by PTFE and ETFE of equal mass, respectively.

[0046] Embodiment 6-7

[0047] The other conditions are the same as those in Example 1, except that in step (S5), the water vapor activation time is different, namely 4 h and 6 h.

[0048] Example 8

[0049] The other conditions are the same as those in Example 1, except that in step (S5), CO2 activation is used instead, Ar is introduced as a protective gas, the temperature is raised to 900°C, CO2 is introduced at a rate of 14.4L CO2 / 1kg of composite secondary carbon particles, and the activation reaction is carried out for 8 hours.

[0050] Example 9

[0051] The other conditions are the same as those in Example 1, except that in step (S5), the KOH solid particles are ground, KOH is added according to a raw material: KOH mass ratio of 1:3, and placed in a rotary furnace; argon is introduced as a protective gas, the temperature is raised to 500° C. and maintained for 1 h, then raised to 850° C. and maintained for 2 h, cooled to 500° C., and water vapor is introduced according to 15 L water vapor / 1 kg of composite secondary carbon particles.

[0052] Example 10

[0053] The other conditions are the same as those in Example 1, except that in step (S1), the amount of PVDF added is 5% of the total mass of the hard carbon and the soft carbon.

[0054] Comparative Example 1

[0055] The other conditions are the same as those in Example 1, except that in step (S1), no carbon nanotubes are added.

[0056] Comparative Example 2

[0057] The other conditions are the same as those in Example 1, except that in step (S1), no phenolic resin is added.

[0058] Comparative Example 3

[0059] The other conditions are the same as those in Example 1, except that in step (S1), PVDF is not added.

[0060] Comparative Example 4

[0061] The other conditions are the same as those in Example 1, except that in step (S1), no soft carbon is added.

[0062] Figure 1 This is the nitrogen adsorption curve of the porous carbon prepared in Example 1.

[0063] Figure 2 This is the pore size distribution diagram of the porous carbon prepared in Example 1.

[0064] The iPore620 full-function gas adsorption instrument produced by Lihua Lianke was used to test the specific surface area, pore volume and pore size of the composite functional porous carbon.

[0065] The preparation process parameters of the porous carbon obtained in the above examples and comparative examples are listed in Table 1, and the characterization data are listed in Table 2.

[0066] Table 1 Process parameters

[0067]

[0068] Table 2 Characterization data

[0069]

[0070] from Figure 1 , Figure 2 It can be seen that the specific expression of the composite functional porous carbon reaches 1822 cm 2 / g, and has 0.93cm 3 / g pore volume and a most probable pore size of 2.75nm. The large pore volume provides a place for silicon deposition, and the pore size of the porous carbon can be adjusted according to the different ratios of soft and hard carbon in Examples 1-3 in Table 1. This is because during the high-temperature activation process, the hard carbon precursor is a thermosetting material, which is difficult to convert into a graphite structure at high temperatures, so its structure is more disordered, contains abundant micropores, and the material also has a larger interlayer distance and is easier to activate and etch to form pores; while the precursor of the soft carbon is a thermoplastic material, which is easier to convert into a graphite structure at high temperatures, with a more ordered structure and a narrower interlayer distance. The activation etching effect under the same conditions is not as good as that of hard carbon. Hard carbon and soft carbon have different degrees of reaction to activating substances such as water vapor, carbon dioxide and KOH at high temperatures, resulting in changes in pore volume and pore size, and then the ratio of the soft and hard carbon precursors is adjusted according to the different specific surfaces, pore volumes and pore sizes of the required porous carbon.

[0071] Figure 3 This is a high-resolution XPS image of the F element of the porous carbon prepared in Example 1. The addition of the F element can be effectively detected. As shown in Tables 2 and 3, the presence of the fluorine element was detected in Examples 1, 4, and 5, indicating that the addition of fluorine-containing resins such as PVDF, PTEE, and ETFE can effectively increase the F content in the porous carbon, and the F element can promote the stable formation of the fluorine-containing electrolyte-negative electrode SEI film and improve the first effect.

[0072] According to the different water vapor activation times of Examples 1, 6, and 7, the water vapor intake per unit time and the temperature, the porous carbon pore size is stably controlled at about 2.75 nm, the activation time is extended from 4 h to 8 h, and the specific surface area is increased from 1105 cm 2 / g increased to 1822cm 2 / g, pore volume from 0.59cm 3 / g increased to 0.93cm 3 / g. Examples 8 and 9 were activated with CO2 and KOH respectively, and both obtained porous carbon materials with high specific surface area and large pore volume. In particular, Example 9 was first activated with KOH and then activated with water vapor, and the specific surface area was the largest.

[0073] Figure 4 This is a 10 MPa-100 MPa four-terminal powder resistivity diagram of the porous carbon prepared in Example 1.

[0074] Figure 5 This is a 10 MPa-100 MPa four-terminal powder resistivity graph of the porous carbon prepared in Comparative Example 1.

[0075] Figure 4 , Figure 5The resistivity curves of porous carbon prepared in Example 1 and Comparative Example 1 at 10MPa-100MPa are shown respectively. The composite functional porous carbon with superP and carbon nanotubes has an average powder resistivity of 0.078Ω·cm at 10MPa-100MPa, which is 0.098Ω·cm compared to the average powder resistivity of 0.098Ω·cm without carbon nanotubes. The combined addition of superP and carbon nanotubes can effectively improve the conductivity of the active material. The addition of carbon nanotubes improves the bonding strength of the battery pole piece and reduces the amount of binder used. At the same time, carbon nanotubes, as a high aspect ratio conductive additive, can build a large-scale conductive network inside the battery, thereby preventing the electrode material in the lithium battery from repeatedly expanding and contracting during the charge and discharge process, and even cracking and cracking. Carbon nanotubes also have extremely high intrinsic thermal conductivity, which can improve the thermal conductivity and heat dissipation of battery poles; carbon nanotubes form liquid diffusion channels inside battery poles, which can also promote the wettability and uniform and rapid penetration of electrolytes in battery poles; carbon nanotubes form a good conductive network inside lithium batteries, which can improve the high-rate charge and discharge capabilities of lithium batteries. The use of carbon nanotubes can reduce the amount of carbon black conductive agents and binders used, increase the proportion of negative electrode materials in the battery, and thus can also increase the energy density of some batteries.

[0076] Figure 6 This is the SEM image of the porous carbon prepared in Example 1.

[0077] Figure 7 This is the SEM image of the porous carbon prepared in Comparative Example 2.

[0078] from Figure 6 , Figure 7 It can be seen that the porous carbon with phenolic resin added in Example 1 has a higher sphericity, while the sphericity of Comparative Example 2 is poor without adding phenolic resin. This is because the resin undergoes a polycondensation reaction during the curing process, and the groups on the C chain continuously fall off during the polycondensation process, causing the C chain to shrink and form a spherical or quasi-spherical shape under the action of internal stress. The regularly shaped sphere can better protect the contact between the silicon material and the electrolyte after silicon deposition and surface carbon coating, while increasing the packing density and increasing the content of active substances per unit area.

[0079] Application Examples

[0080] The porous carbon prepared in the above embodiments and comparative examples was used as a carbon source for CVD vapor deposition. Specifically, 1 kg of porous carbon was first placed in a rotary kiln, and Ar was introduced as a protective gas. The rotary kiln speed was 60 r / min. The temperature rose to 500 ° C and remained stable. Then, silane gas was introduced at a flow rate of 3 L / min for 4.5 hours. Silane was cracked into Si and deposited in the voids of the porous carbon. After the silicon-carbon material was formed, the introduction of silane gas was stopped. Then, the temperature was raised to 900 ° C, and acetylene gas was introduced at a flow rate of 3 L / min for 2 hours. Acetylene was cracked into carbon coated on the surface of the deposited silicon-carbon to form an active substance of the negative electrode material of a lithium battery. The obtained silicon-carbon active material was used as the negative electrode of the battery for electrochemical testing. Specifically, the active material, polyacrylic acid (PAA), and superP were mixed in deionized water at a mass ratio of 8: 1: 1, and after being fully ground, they were placed in a homogenizer to prepare a slurry. Then, the slurry was evenly coated on the copper foil at a thickness of 200um and placed in a vacuum drying oven for drying. Subsequently, a 12mm pole piece was made by a punching machine and placed in a vacuum glove box, a 16mm lithium sheet was selected as a symmetrical electrode, Celgard2600 was selected, and it was cut into 18mm as a diaphragm, and a 1M LiPF6 electrolyte of Kelude (the solvent was 1:1:1 by volume ratio of EC:EDC:EMC, and 5% FEC was added) was selected to prepare a CR2032 button battery. A blue electric system was used for electrochemical testing. Specifically, the battery was left to stand for 1 hour, then discharged at a rate of 0.1C until the voltage dropped to 0.005V, then left to stand for 1 hour, then discharged at a rate of 0.02C until the voltage dropped to 0.005V, then left to stand for 1 hour, then discharged at a rate of 0.01C until the voltage dropped to 0.005V, then charged at a rate of 0.1C until the voltage reached 1.5V and then stopped.

[0081] Figure 8 The XRD spectrum of Example 1 after CVD deposition shows that there are only two materials, silicon and carbon, in the composite functional porous carbon material. It can be analyzed from Table 3 that the difference in specific surface area, pore volume and pore size will affect the deposition degree of porous carbon on silicon material, thereby affecting the overall electrochemical performance.

[0082] Fig. 9 This is the first cycle charge and discharge curve of the negative electrode material prepared from the porous carbon in Example 1, which shows that the first efficiency at 1.5V can reach 93.1%. By comparing the capacity and first efficiency of the embodiment with those of comparative examples 1-4, it is shown that the sphericity of the composite functional porous carbon, the addition of graphite and carbon nanotubes, the addition of F elements, and the combination of hard carbon and soft carbon all improve the electrochemical properties of the silicon-carbon composite negative electrode material.

[0083] The porous carbon of the above-mentioned embodiment and comparative example was prepared as negative electrode material according to the above-mentioned method, and then the electrochemical performance data was measured. The results are shown in Table 3.

[0084] Table 3 Electrochemical performance data test

[0085]

[0086]

Claims

1. A method for preparing a porous carbon material with gradient pore size, characterized in that: The following steps are involved: (S1) crushing soft carbon and hard carbon to disperse in solvent, adding phenolic resin and fluorine-containing resin; (S2) adding micron-sized conductive carbon material and carbon nanotube material to obtain a suspension; (S3) spraying and granulating the suspension to obtain a secondary particle precursor with a D50 of 5-10 μm, and drying for later use; (S4) curing the dried secondary particle precursor with a phenolic resin at 160-200° C. under a protective atmosphere, and then heating it to 500-600° C. for carbonization to obtain composite secondary carbon particles; (S5) The composite secondary carbon particles are activated to form pores to obtain a porous carbon material with a gradient pore size.

2. The preparation method according to claim 1, characterized in that: In step (S1), the hard carbon is selected from at least one of biomass pyrolysis carbon and polymer pyrolysis carbon; the soft carbon is selected from at least one of asphalt, petroleum coke, and needle coke; the hard carbon accounts for 30-70wt% of the total mass of the hard carbon and the soft carbon, preferably 50-70%.

3. The preparation method according to claim 2, characterized in that: The biomass pyrolytic carbon is selected from coconut shell charcoal, straw charcoal and bamboo; the polymer pyrolytic carbon is selected from phenolic resin carbide and epoxy resin carbide.

4. The preparation method according to claim 1, characterized in that: In step (S1), the solvent is selected from at least one of ethanol, N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), and dimethyl sulfoxide (DMSO), and the amount of solvent added is sufficient to achieve full dissolution.

5. The preparation method according to claim 1, characterized in that: In step (S1), the molecular weight of the phenolic resin is 5000-100000, and the fluorine-containing resin is selected from at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), and ethylene-tetrafluoroethylene copolymer (ETEE); the amount of the phenolic resin added is 10-20% of the total mass of the soft carbon and the hard carbon, and the amount of the fluorine-containing resin added is 5-10% of the total mass of the soft carbon and the hard carbon.

6. The preparation method according to claim 1, characterized in that: In step (S2), the micron-sized conductive carbon material is selected from at least one of Super P and conductive carbon black, and the size of the micron-sized conductive carbon material is 1-3 μm.

7. The preparation method according to claim 1, characterized in that: The amount of micron-grade conductive carbon material added is 10-15% of the total mass of hard carbon and soft carbon; the amount of carbon nanotube material added is 0.5-2% of the total mass of hard carbon and soft carbon.

8. The preparation method according to claim 1, characterized in that: In step (S3), the process parameters of the spray granulation are that the pressure is controlled at 0.08-0.1 MPa, the feed rate is controlled at 100-300 mL / min, and the D50 of the obtained secondary carbon sphere particles is 5-10 μm; High temperature curing is a treatment at 700-1000° C. for 2-5 hours in a carbonization inert atmosphere; preferably, the inert atmosphere is at least one of nitrogen, argon and helium.

9. The preparation method according to claim 1, characterized in that: In step (S5), the pore-forming activation is physical activation or chemical activation. The physical activation uses water vapor or carbon dioxide as an activator, and the physical activation is carried out at 800-1000°C, preferably 900-1000°C; the chemical activation is alkali activation, that is, activation is carried out under KOH and / or NaOH conditions, and the alkali activation is carried out at 750-900°C.

10. Use of the porous carbon material prepared by the preparation method according to any one of claims 1 to 9 in the preparation of silicon-carbon negative electrode materials.

Citation Information

Patent Citations

  • High-capacity ratio rate carbon-based composite material, preparation method thereof and application thereof in lithium ion battery

    CN107768626A

  • Composite hard carbon material and preparation method and application thereof

    CN115911320A

  • Silicon-based negative electrode material, silicon electrode and lithium ion battery

    CN116230885A

  • Negative pole piece, lithium ion battery and electronic device

    CN117038855A

  • Method for preparing boron-doped porous carbon sphere

    WO2017190677A1

Cited By

  • Porous carbon with secondary particle configuration, preparation method and application of porous carbon, gas-phase silicon carbon material and application of gas-phase silicon carbon material

    CN119143129A

  • Preparation method of porous carbon adaptive to non-expansion silicon-carbon negative electrode battery

    CN119706787A

  • Activated carbon, silicon-carbon composite material and preparation method and application thereof

    CN119706832A

  • Spherical porous carbon as well as preparation method and application thereof

    CN119976806A

  • Method for preparing porous carbon through secondary utilization of fine powder of porous carbon airflow powder

    CN120589750A