Barrier film with lasting space maintenance and preparation method thereof

By using animal tissue stacking and an intermediate layer of collagen and manganese in the barrier film, the problem of degradation and rupture of the existing barrier film in the body is solved, the mechanical strength is improved, long-lasting space maintenance is achieved, and the requirements for dental implants are met bone regeneration needs.

CN118787791APending Publication Date: 2024-10-18XILING (ZHENJIANG) MEDICAL TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410952321.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The existing barrier membrane is prone to rupture during the degradation process in the body, and its mechanical strength is insufficient, which affects the bone regeneration effect.

Method used

The animal tissue is stacked and an intermediate layer containing collagen and manganese is added to form a barrier film with long-lasting space maintenance. By stacking layers, it enhances mechanical strength and promotes bone cell reproduction and adhesion.

Benefits of technology

It effectively avoids the rupture of the barrier film during the degradation process in the body, and at the same time improves the mechanical strength, with a tensile strength of up to 61.70MPa, meeting the needs of the oral environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118787791A_ABST
    Figure CN118787791A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of oral isolating membranes, and discloses a barrier membrane with lasting space maintenance and a preparation method thereof. The disclosed barrier membrane comprises: animal tissue; animal tissues are subjected to stacking treatment, and a middle layer is contained in a stacked layer. The preparation method comprises the following steps: degreasing and deproteinizing animal tissues A for later use; putting animal tissues B into an acetic acid solution to extract collagen, dialyzing the solution with purified water, pouring manganese powder into the solution after dialysis is completed, and uniformly stirring to obtain a mixed solution; pouring the mixed solution into a mold for freeze-drying to obtain a middle layer; spreading the spare animal tissues, overlapping a plurality of layers, and adding a middle layer in the process; after the working procedure is finished, each layer is compacted into a thin sheet, and freeze-drying is carried out; and after freeze-drying, packaging and sterilizing. According to the barrier film and the preparation method thereof, the phenomenon that the barrier film is degraded and broken in vivo during use is avoided, and meanwhile the mechanical strength of the barrier film is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oral isolation membranes, and in particular relates to a barrier membrane with long-lasting space maintenance and a preparation method thereof. Background Art

[0002] Tooth loss caused by accidental trauma, long-term tooth loss, severe periodontitis and other factors will cause progressive resorption of the alveolar bone, resulting in a decrease in the height and narrowing of the alveolar ridge, affecting the quality of bone integration after implant placement, and hindering the retention and stability of implant dentures.

[0003] In the past, autologous iliac bone and fibula transplantation technology was often used to solve the problem of insufficient bone mass. However, this method causes surgical trauma to the bone donation area and may induce complications such as postoperative infection. Currently, guided bone regeneration technology has been experimentally and clinically proven to effectively solve the problem of insufficient bone mass encountered in dental implant surgery.

[0004] The membrane regeneration technology for bone tissue is defined as GBR technology. Dahlin et al. conducted a mouse mandibular angle bone defect healing experiment using polytetrafluoroethylene membranes and found that complete bone tissue regeneration was observed on the membrane-covered side, while almost no bone tissue regeneration was observed on the non-membrane-covered side. The guided bone regeneration membrane is the key to this technology and plays an important role in the bone tissue repair process.

[0005] Depending on whether the membrane can be absorbed in the body, it is divided into non-absorbable membrane and absorbable membrane.

[0006] The non-absorbable membrane can determine the duration of its stay in the body according to the specific situation of bone defect healing, but its poor tissue affinity will lead to wound infection and cracking, affecting the quality of bone regeneration. Because it is non-degradable, a second surgery is required, which will damage the repaired gingival tissue, increase the risk of infection, and cause more pain to the patient.

[0007] The current absorbable membrane has good biocompatibility, low antigenicity and is degradable. However, the mechanical strength of the absorbable membrane is low and it cannot maintain the space required for bone regeneration for a long time. During the degradation process in the body, it will break, which is often manifested as: the suture is not degraded, but the membrane covering the defect has degraded and broken (that is, the middle part degrades and breaks first, and the surrounding area is not degraded, which affects the use effect). Summary of the invention

[0008] In view of the problem that barrier membranes currently break during degradation in the body, the present invention aims to provide a barrier membrane with long-lasting spatial maintenance and a preparation method thereof, thereby avoiding degradation and rupture of the barrier membrane in the body during use, while improving the mechanical strength of the barrier membrane.

[0009] The object of the present invention is to provide a barrier film with long-lasting space maintenance, the barrier film comprising: animal tissue; the animal tissue is stacked, and the stacked layers contain an intermediate layer.

[0010] Furthermore, the animal tissue is selected from any one of the pericardium, dermis, and submucosa of pigs, cattle, or sheep.

[0011] Furthermore, the middle layer contains collagen and manganese.

[0012] A method for preparing a barrier film with long-lasting space maintenance, the preparation method comprising the following steps:

[0013] (1) taking animal tissue A, defatting and deproteinizing it for later use;

[0014] (2) taking animal tissue B and placing it in an acetic acid solution to extract collagen, dialyzing the solution with purified water, and after the dialysis is completed, pouring manganese powder into the solution, stirring it evenly to obtain a mixed solution;

[0015] (3) pouring the mixed solution into a mold and freeze-drying to obtain an intermediate layer;

[0016] (4) Spreading the animal tissue prepared in step (1) and stacking several layers, adding 1 to 2 intermediate layers at a time during this process; after the process is completed, compacting each layer into a thin sheet and freeze-drying;

[0017] (5) After freeze-drying, packaging and sterilization with cobalt 60, it is ready.

[0018] Furthermore, in the step (2), the mass ratio of manganese powder to collagen is 1-2:3000-5000.

[0019] Furthermore, the volume fraction of acetic acid in step (2) is 0.15%-0.5%.

[0020] Furthermore, the intermediate layer obtained in step (3) is adjusted and cut according to the required size of the barrier film when in use, and has a thickness of 0.02-0.04 mm.

[0021] Furthermore, the number of stacked layers in step (4) is 15 to 20 layers.

[0022] Furthermore, the stacking method adopts a layer-by-layer stacking method, first laying out a layer, and then laying out a second layer and stacking it thereon, and stacking several layers; the defatted and deproteinized animal tissue A is adjusted and cut according to the required size of the barrier membrane for stacking.

[0023] Compared with the prior art, the advantages of the present invention are:

[0024] The present invention and common barrier membranes use the same material, animal tissue, but the difference is that collagen is extracted from the tissue to make an intermediate layer, which is used to be spread on the stacked layers of pre-defatted and deproteinized animal tissue. First, the source of raw materials is convenient, taken from animal tissue and used on animal tissue; secondly, manganese powder is added to the collagen solution to regulate the interaction between extracellular matrices, thereby promoting bone cell reproduction, adhesion and diffusion, and obtaining an intermediate layer, which is sandwiched in the defatted and deproteinized animal tissue, can greatly improve osteogenic inductivity and biocompatibility; experiments have shown that the barrier membrane prepared by the present application can avoid rupture during degradation in the body, and at the same time improve the mechanical strength of the barrier membrane; after testing, the tensile strength of the barrier membrane can reach 61.70MPa, which can well meet the use requirements and is not prone to rupture in the oral environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 , 2 3 are photos of the barrier film obtained in Example 1 after the degradation test, corresponding to the degradation conditions after 1d, 15d, and 27d respectively;

[0026] Figure 4 , 5 , 6 are photographs of the barrier film obtained in Example 2 after degradation test, corresponding to the degradation conditions after 1d, 20d, and 30d, respectively. DETAILED DESCRIPTION

[0027] The following provides a specific embodiment of a barrier film with a persistent space-maintaining property and a preparation method thereof. It is necessary to point out that the following examples are only used to explain the present invention in more detail, rather than to narrow the scope of protection of the present invention. After reading the present invention, improvements and adjustments made by professionals in this technical field without departing from the concept of the present invention are within the scope of protection claimed by the present invention.

[0028] Example 1

[0029] A method for preparing a barrier film with long-lasting space maintenance, the preparation method comprising the following steps:

[0030] (1) taking animal tissue A, defatting and deproteinizing it for later use;

[0031] (2) taking animal tissue B and placing it in an acetic acid solution to extract collagen, dialyzing the solution with purified water, and after the dialysis is completed, pouring manganese powder into the solution, stirring it evenly to obtain a mixed solution;

[0032] (3) pouring the mixed solution into a mold and freeze-drying to obtain an intermediate layer;

[0033] (4) Spreading out the animal tissue prepared in step (1) and stacking several layers, adding two or three intermediate layers at a time during this process; after the process is completed, compacting each layer into a thin sheet and freeze-drying;

[0034] (5) After freeze-drying, packaging and sterilization with cobalt 60, it is ready.

[0035] Wherein, in step (2), the mass ratio of manganese powder to collagen is 1:3000.

[0036] Wherein, the volume fraction of acetic acid in step (2) is 0.25%.

[0037] The intermediate layer obtained in step (3) is adjusted and cut according to the required size of the barrier film when in use, and has a thickness of 0.03 mm.

[0038] Among them, the number of stacked layers in step (4) is 20.

[0039] Among them, the stacking method adopts a layer-by-layer stacking method, first laying a layer flat, and then laying a second layer flat and stacking it, and stacking several layers; the animal tissue A that has been defatted and deproteinized is adjusted and cut according to the required size of the barrier membrane for stacking.

[0040] Example 2

[0041] A method for preparing a barrier film with long-lasting space maintenance, the preparation method comprising the following steps:

[0042] (1) taking animal tissue A, defatting and deproteinizing it for later use;

[0043] (2) taking animal tissue B and placing it in an acetic acid solution to extract collagen, dialyzing the solution with purified water, and after the dialysis is completed, pouring manganese powder into the solution, stirring it evenly to obtain a mixed solution;

[0044] (3) pouring the mixed solution into a mold and freeze-drying to obtain an intermediate layer;

[0045] (4) Spreading out the animal tissue prepared in step (1) and stacking several layers, adding two or three intermediate layers at a time during this process; after the process is completed, compacting each layer into a thin sheet and freeze-drying;

[0046] (5) After freeze-drying, packaging and sterilization with cobalt 60, it is ready.

[0047] Wherein, in step (2), the mass ratio of manganese powder to collagen is 1:4000.

[0048] Wherein, the volume fraction of acetic acid in step (2) is 0.25%.

[0049] The intermediate layer obtained in step (3) is adjusted and cut according to the required size of the barrier film when in use, and has a thickness of 0.03 mm.

[0050] Among them, the number of stacked layers in step (4) is 20.

[0051] Among them, the stacking method adopts a layer-by-layer stacking method, first laying a layer flat, and then laying a second layer flat and stacking it, and stacking several layers; the animal tissue A that has been defatted and deproteinized is adjusted and cut according to the required size of the barrier membrane for stacking.

[0052] Comparative Example 1: It is basically the same as Example 1, except that the middle layer is missing.

[0053] Comparative Example 2: The same as Example 1, except that manganese powder is missing.

[0054] Comparative Example 3: Commercially available dental barrier film (main component: polylactic acid).

[0055] Examples 1 to 2 and Comparative Examples 1 to 3 were tested to determine tensile strength and degradation tests.

[0056] Tensile strength test method: Test according to the method specified in GB / T 1040.3-2006.

[0057] Degradation test: Use 0.02mg / mL collagenase solution at 37℃ and 50% humidity to simulate the product use environment. Figure 1 , 2 3 are photos of the barrier film obtained in Example 1 after the degradation test, corresponding to the degradation conditions after 1d, 15d, and 27d respectively; Figure 4 , 5 , 6 are photos of the Example 2 group after the degradation test, corresponding to the degradation conditions after 1d, 20d, and 30d, respectively.

[0058] Table 1. Test results

[0059] Group Tensile strength / MPa Example 1 61.7 Example 2 61.4 Comparative Example 1 51.3 Comparative Example 2 57.2 Comparative Example 3 42.6

[0060] From the data of tensile strength, it can be seen that the lack of the middle layer in comparative example 1 leads to a significant decrease in tensile strength, the lack of manganese powder in comparative example 2 leads to a certain degree of decline in tensile strength, and the tensile resistance of comparative example 3 is relatively weak. From the degradation test pictures, it can be seen that both groups of examples can degrade evenly, and the common situation of degradation and rupture of the middle part first, which affects the test effect, does not occur.

[0061] Note: The above embodiments are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention; therefore, although this specification has described the present invention in detail with reference to the above embodiments, a person skilled in the art should understand that the present invention can still be modified or replaced by equivalents; and all technical solutions and improvements thereof that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A barrier film with long-lasting space maintenance, characterized in that: The barrier membrane comprises: animal tissue; the animal tissue is stacked, and the stacked layers contain an intermediate layer.

2. The barrier film with long-lasting space maintenance according to claim 1, characterized in that: The animal tissue is selected from any one of the pericardium, dermis, and submucosa of pigs, cattle, or sheep.

3. The barrier film with long-lasting space maintenance according to claim 1, characterized in that: The middle layer contains collagen and manganese.

4. A method for preparing a barrier film having a long-lasting space-maintaining property as claimed in claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) taking animal tissue A, defatting and deproteinizing it for later use; (2) taking animal tissue B and placing it in an acetic acid solution to extract collagen, dialyzing the solution with purified water, and after the dialysis is completed, pouring manganese powder into the solution, stirring it evenly to obtain a mixed solution; (3) pouring the mixed solution into a mold and freeze-drying to obtain an intermediate layer; (4) Spreading the animal tissue prepared in step (1) and stacking several layers, adding 1 to 2 intermediate layers at a time during this process; after the process is completed, compacting each layer into a thin sheet and freeze-drying; (5) After freeze-drying, packaging and sterilization with cobalt 60, it is ready.

5. The method for preparing a barrier film with long-lasting space maintenance according to claim 4, characterized in that: In the step (2), the mass ratio of manganese powder to collagen is 1-2:3000-5000.

6. The method for preparing a barrier film having a long-lasting space-maintaining property according to claim 4, characterized in that: The volume fraction of acetic acid in step (2) is 0.15%-0.5%.

7. The method for preparing a barrier film with long-lasting space maintenance according to claim 4, characterized in that: The intermediate layer obtained in step (3) is adjusted and cut according to the required size of the barrier film when in use, and has a thickness of 0.02-0.04 mm.

8. The method for preparing a barrier film with long-lasting space maintenance according to claim 4, characterized in that: The number of stacked layers in step (4) is 15 to 20 layers.

9. The method for preparing a barrier film with long-lasting space maintenance according to claim 4, characterized in that: The stacking method adopts a layer-by-layer stacking method, first laying out a layer, and then laying out a second layer and stacking it thereon, and stacking several layers; the defatted and deproteinized animal tissue A is adjusted and cut according to the required size of the barrier membrane for stacking.