Methane combustion catalyst with high stability and preparation method thereof
By loading Mn-Co solid solution on Ce-Ti oxide, constructing a stacked structure and oxygen vacancy engineering, the problems of spinel oxide activity regulation and insufficient metal-support interaction are solved, and high stability and low-temperature activity are achieved. Methane combustion catalyst with high water and sulfur dioxide resistance.
Patent Information
- Application Number
- CN202410932971.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-12
AI Technical Summary
Existing methane combustion catalysts have challenges in long-term stability and resistance to toxicity, especially insufficient activity control and metal-support interaction of spinel oxides, resulting in unsatisfactory catalytic stability.
Ce-Ti oxide is prepared by co-precipitation method as a carrier, and Mn-Co solid solution is loaded on it. The stability and activity of the catalyst are improved by constructing a stacked structure and oxygen vacancy engineering, and Ti-induced CeO2 crystal reconstruction is used to form SO2. Strong affinity site, enhanced sulfur resistance and oxygen migration ability.
The catalyst achieves high stability and excellent low-temperature activity, can reach 90% methane conversion rate at 400°C, and has high water resistance and sulfur dioxide resistance, significantly improving catalytic oxidation activity and anti-poisoning performance.
Smart Images

Figure CN118788356A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of energy and environmental technology, and in particular to a methane combustion catalyst with high stability and a preparation method thereof. Background Art
[0002] There is a highly elastic CH bond in the CH4 molecule (the bond energy is about 435 kJ·mol -1 ), which makes its degradation very difficult. The traditional methane flame combustion temperature must be above 1500℃, and it will also react with N2 in the air to produce NO x Pollutants are extremely harmful to the environment. Moreover, the energy utilization rate of traditional flame combustion is very low, which is not suitable for energy-saving and environmentally friendly treatment. Therefore, changing the combustion method of methane is the key issue at present, and catalytic oxidation has the advantages of moderate operating temperature and high removal efficiency, which is an economical and effective method to reduce the emission of unburned methane and CO.
[0003] For the catalytic combustion of methane, its catalysts can be divided into two categories: precious metal catalysts and non-precious metal catalysts. At present, researchers have made great progress in the study of precious metals, and have achieved certain research results in both preparation methods and reaction mechanisms. Although precious metal catalysts show significant activity, their widespread adoption is hindered by their high cost and easy poisoning. As for non-precious metal catalysts, especially transition metal oxide catalysts (TMOs), they have attracted great attention due to their low cost and good activity, and the advantages of variable valence and adjustable occupied orbitals in redox reactions. However, the activity of transition metal oxide catalysts is still significantly different from that of precious metal catalysts. Therefore, improving the catalytic efficiency of transition metal oxide catalysts is crucial to promote the application of deep oxidation technology in mitigating light alkane emissions.
[0004] The reported catalytic systems mainly include Mn-based, Ce-based, Cu-based, Fe-based and multi-element composite catalyst systems. 3+ and Mn 4+ There may be double exchange behavior between them, and they have unique catalytic redox properties. Therefore, Mn-based materials contain a large amount of surface active oxygen, which has attracted much attention in the study of catalytic oxidation. In particular, the Mn-based spinel structure refers to the AB2O4 composition (where A and B are metal ions in tetrahedral and octahedral positions, respectively), which has excellent reducibility, strong surface acidity, high surface oxygen concentration and structural stability. Spinel catalysts contain a large amount of active oxygen and abundant acid sites. Studies have found that oxygen vacancies on cobalt manganese spinel are an important active site for redox reactions. Oxygen vacancies can increase the mobility and activity of lattice oxygen through the transport effect, which promotes the reduction and electron migration of the catalyst. This may be due to the stable three-dimensional structure of spinel, which protects the active sites.
[0005] However, there are still some obstacles to long-term stable methane catalytic reaction, which is also the problem faced by current methane combustion catalysts. Regulating the activity of oxygen on spinel oxides to improve their catalytic activity has always been a challenge for heterogeneous catalytic oxidation reactions; at the same time, due to the lack of appropriate metal-support interactions and anti-toxic sites, metal active components are easily aggregated and poisoned by SO2 and H2O for a long time at low temperatures, resulting in unsatisfactory catalytic stability.
[0006] The chemical etching effect of urea at high temperature can be used to construct and adjust oxygen vacancies. As the concentration of oxygen vacancies increases, the catalytic oxidation activity of various VOCs is significantly enhanced, which is comparable to the original Co x Mn 3-x Compared with O4 spinel catalysts, the dual activation of lattice oxygen and gaseous molecular oxygen has been significantly promoted due to the modification of oxygen vacancy engineering, which has practical significance in the field of environmental catalysis.
[0007] Supported catalysts have become the mainstream catalysts due to their low cost, improved thermal stability, sulfur resistance and other properties, as well as their higher catalytic activity compared to pure substance catalysts or solid solution catalysts. However, different types of supports have a great influence on the activity, stability and other properties of the catalyst.
[0008] Therefore, developing a high-performance methane combustion catalyst with excellent low-temperature activity and high resistance to heat and poisoning and a preparation method thereof through interface engineering is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0009] In view of this, the present invention provides a methane combustion catalyst with high stability and a preparation method thereof.
[0010] To achieve the above object, the present invention adopts the following technical solutions:
[0011] A method for preparing a methane combustion catalyst with high stability comprises the following steps:
[0012] (1) Preparation of Ce-Ti oxide by coprecipitation method
[0013] C 12 H 28 O4Ti was dissolved in ethanol, and then Ce(NO3)3·6H2O was added to the solution and stirred for reaction. Then, the pH was adjusted with ammonia water, and the mixture was stirred for 2-4 hours. After aging for 2-4 hours, the precipitate was filtered and washed with water. The washed precipitate was dried and then heated in flowing air to obtain nanostructured Ce. xTi 1-x O2 carrier, i.e. Ce-Ti oxide, Ce x Ti 1-x O2 wherein x = 0.1-0.9, preferably 0.5;
[0014] (2) Loading Mn-Co solid solution on Ce-Ti oxide
[0015] (2.1) Loading Mn-Co solid solution on Ce-Ti oxide by positive drop method
[0016] Co(NO3)2·6H2O and Mn(CH3COO)2·4H2O are dissolved in water, which is referred to as solution A. Ce-Ti oxide and ammonium bicarbonate solution are then mixed, which is referred to as solution B. Solution A is slowly dripped into solution B, and after stirring for 1-8 hours, the mixture is filtered, and the precipitate is washed with ethanol and deionized water to a pH of 7-7.5 to obtain a sample. The sample is dried and calcined, urea is added to grind the sample, and the sample is calcined again to obtain a supported X Mn x Co 3-x O4 / Y Ce x Ti 1-x O2 catalyst;
[0017] (2.2) Loading Mn-Co solid solution on Ce-Ti oxide by back-drip method
[0018] Dissolve Co(NO3)2·6H2O, Mn(CH3COO)2·4H2O, and Ce-Ti oxide in water, then slowly drop ammonium bicarbonate solution, precipitate, stir, react, and age for 6-8h, filter, wash with ethanol and deionized water, and precipitate to pH 7-7.5 to obtain a sample. After drying, calcine the sample, add urea to grind, and calcine again to obtain supported X Mn x Co 3-x O4 / Y Ce x Ti 1-x O2 catalyst;
[0019] Load type XMn x Co 3-x O4 / YCe x Ti 1-x O2 catalyst formula: X:Y = 5-8:2-5, Mn x Co 1-x In O4, x=0.1-3, preferably 0.5; Ce x Ti 1-x In O2, x=0.1-0.9, preferably 0.5.
[0020] Furthermore, in step (1), the stirring reaction temperature is 60-80° C., and the stirring reaction time is 20-40 min.
[0021] Furthermore, the mass concentration of the ammonia water in step (1) is 6%, and the ammonia water is dripped into the solution at a dripping rate of 5 mL / min to adjust the pH to 8.5-10.
[0022] Furthermore, the drying temperature in step (1) is 80-100° C. and the drying time is 10-12 h;
[0023] Furthermore, the flowing air heating temperature is 400-500° C., the heating time is 3-4 hours, and the air flow rate is 20-50 ml / min.
[0024] Furthermore, the dropping temperature in step (2.1) is 50-80° C., and the dropping speed is 5 ml / min.
[0025] The concentration of the ammonium bicarbonate solution is 1 mol / L
[0026] Furthermore, the sample drying temperature in step (2.1) is 80-100° C. and the drying time is 6-7 h;
[0027] The sample calcination temperature is 400-500°C and the calcination time is 3-4h;
[0028] The mass ratio of the sample to urea is 1:4;
[0029] The re-calcination temperature is 400-600° C., and the calcination time is 3-4 hours.
[0030] Furthermore, the dropping temperature in step (2.2) is 60-70° C., and the dropping speed is 5 ml / min;
[0031] The concentration of the ammonium bicarbonate solution is 1 mol / L
[0032] Furthermore, the sample drying temperature in step (2.2) is 80-100° C. and the drying time is 6-7 h;
[0033] The sample calcination temperature is 400-500°C and the calcination time is 3-4h;
[0034] The mass ratio of the sample to urea is 1:4;
[0035] The re-calcination temperature is 400-600° C., and the calcination time is 3-4 hours.
[0036] The beneficial effects of the present invention are:
[0037] A layered structure was constructed by loading a Mn-Co-based solid solution catalyst onto Ti-doped CeO2. Two strong SO2 affinity sites were formed through Ti-induced reconstruction of CeO2 crystals, which delayed the influence of sulfate species on the active center, thereby improving stability. The "low-temperature active sites" and "double anti-poisoning sites" give it excellent activity and stability. The layered structure promotes the formation of active metal-support interfaces. The strong interaction between the metal-support interface is conducive to inhibiting the formation of surface adsorbed hydroxyls, and is conducive to oxygen migration (including adsorbed oxygen, lattice oxygen and oxygen vacancies) and metal charge transfer. In addition, by constructing oxygen vacancy engineering (urea modification: chemical etching effect of urea at high temperature) to construct and adjust oxygen vacancies, the catalytic oxidation activity is significantly enhanced as the oxygen vacancy concentration increases. This achieves excellent low-temperature activity of low-concentration methane combustion catalysts, while also having high water resistance and sulfur dioxide resistance stability.
[0038] In the scheme of the present invention, CeO2 has abundant surface oxygen vacancies, which can serve as adsorption and activation sites for SO2, protecting active components from being poisoned. However, pure CeO2 degrades rapidly due to a significant reduction in surface area under high temperature treatment, and cannot meet the requirements of practical use. After doping or surface modification of the present invention, the structural properties of CeO2 can be improved. Introducing other metal ions into the CeO2 lattice to form a solid solution based on CeO2 can make the material have higher oxygen storage capacity, thermal stability and redox performance, thereby having excellent catalytic performance.
[0039] The catalyst prepared by the invention has excellent low-temperature activity, and the conversion rate of ultra-low-concentration methane (methane concentration 0.5%-1.5%) can reach 90% at a temperature of 400°C. It also has high stability in water resistance and sulfur dioxide resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The present invention is a process flow chart for preparing a methane combustion catalyst with high stability;
[0041] Figure 2 100ppm SO2 to 50% Mn at 0.5% methane concentration 0.5 Co 2.5 O4 / 50%Ce 0.5 Ti 0.5 Influence of O2 catalyst on catalytic performance;
[0042] Figure 3 100ppm SO2 to 70% Mn at 1% methane concentration 0.5 Co 2.5 O4 / 30%Ce 0.5 Ti 0.5 Influence of O2 catalyst on catalytic performance;
[0043] Figure 4 100ppm SO2 to 80% Mn at 1.5% methane concentration 0.5 Co 2.5 O4 / 20%Ce 0.5 Ti 0.5 Influence of O2 catalyst on catalytic performance. DETAILED DESCRIPTION
[0044] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] Example 1
[0046] A method for preparing a methane combustion catalyst with high stability:
[0047] (1) Preparation of Ce-Ti oxide by coprecipitation method
[0048] C 12 H 28 O4Ti was dissolved in ethanol, and then Ce(NO3)3·6H2O was added to the solution and stirred at 70°C for 30 minutes. The molar ratio of Ti to Ce was 1:1. Then 6% ammonia water was dripped into the solution at a drip rate of 5 mL / min to adjust the pH to 9. After stirring again for 3 hours, aging for 3 hours, filtering the precipitate and washing with water. The washed precipitate was dried at 90°C for 12 hours, and then heated at 450°C for 3.5 hours in flowing air at a flow rate of 30 ml / min to obtain nanostructured Ce. 0.5 Ti 0.5 O2 carrier, i.e. Ce-Ti oxide;
[0049] (2) Loading Mn-Co solid solution on Ce-Ti oxide by positive drop method
[0050] Co(NO3)2·6H2O and Mn(CH3COO)2·4H2O were dissolved in water, the molar ratio of Mn to Co was 1:5, and the sample was Mn 0.5 Co 2.5 O4, recorded as solution A, and then Ce 0.5 Ti 0.5O2 and 400ml of 1mol / L ammonium bicarbonate solution were mixed, which was recorded as solution B; solution A was slowly dripped into solution B at a rate of 5ml / min at 65°C, stirred for reaction and aging for 4h, filtered, washed with ethanol and deionized water, and the precipitate was pH 7 to obtain a sample; the sample was dried at 100°C for 6h, then calcined at 450°C for 3.5h, urea 4 times the mass of the sample was added for grinding, and calcined again at 500°C for 3.5h to obtain a supported 50% Mn 0.5 Co 2.5 O4 / 50%Ce 0.5 Ti 0.5 O2 catalyst.
[0051] Example 2
[0052] A method for preparing a methane combustion catalyst with high stability:
[0053] (1) Preparation of Ce-Ti oxide by coprecipitation method
[0054] C 12 H 28 O4Ti was dissolved in ethanol, and then Ce(NO3)3·6H2O was added to the solution and stirred at 70°C for 30 minutes. The molar ratio of Ti to Ce was 1:1. Then 6% ammonia water was dripped into the solution at a drip rate of 5 mL / min to adjust the pH to 9. After stirring again for 3 hours, aging for 3 hours, filtering the precipitate and washing with water. The washed precipitate was dried at 90°C for 12 hours, and then heated at 450°C for 3.5 hours in flowing air at a flow rate of 30 ml / min to obtain nanostructured Ce. 0.5 Ti 0.5 O2 carrier, i.e. Ce-Ti oxide;
[0055] (2) Loading Mn-Co solid solution on Ce-Ti oxide by back-drip method
[0056] Co(NO3)2·6H2O, Mn(CH3COO)2·4H2O, and Ce-Ti oxide were dissolved in water, with a molar ratio of Mn to Co of 1:5, and then 400 ml of 1 mol / L ammonium bicarbonate solution was slowly dripped at a rate of 5 ml / min at 65°C. After the precipitation was stirred and aged for 7 hours, it was filtered and washed with ethanol and deionized water to obtain a sample with a pH of 7. The sample was dried at 100°C for 6 hours, and then calcined at 450°C for 3.5 hours. Urea 4 times the mass of the sample was added for grinding, and calcined again at 500°C for 3.5 hours to obtain a supported 50% Mn 0.5 Co 2.5 O4 / 50%Ce 0.5 Ti 0.5 O2.
[0057] Example 3
[0058] The preparation steps are basically the same as those in Example 1. The difference from Example 1 is that the ratio of Co(NO3)2·6H2O, Mn(CH3COO)2·4H2O and Ce-Ti oxide is adjusted to prepare a product with a supported 70% Mn 0.5 Co 2.5 O4 / 30%Ce 0.5 Ti 0.5 O2.
[0059] Example 4
[0060] The preparation steps are basically the same as those in Example 1. The difference from Example 1 is that the ratio of Co(NO3)2·6H2O, Mn(CH3COO)2·4H2O and Ce-Ti oxide is adjusted, and the prepared product is a supported 80% Mn 0.5 Co 2.5 O4 / 20%Ce 0.5 Ti 0.5 O2.
[0061] Test Example 1
[0062] As in Example 1, Mn 0.5 Co 2.5 O4 and Ce 0.5 Ti 0.5 O2 was loaded 1:1, recorded as 50% Mn 0.5 Co 2.5 O4 / 50%Ce 0.5 Ti 0.5 O2; the catalyst was placed in a fixed bed reactor and stability tested at a methane concentration of 0.5%; the temperature was programmed from 0 to 500°C, the reaction raw gas ratio was 0.5% methane, 20% O2, and the rest was Ar, the space velocity was 45000mL / (gh), and the methane conversion rate was observed; 100ppm SO2 was introduced on the basis of the raw gas, and the change in methane conversion rate was observed. The results are as follows Figure 2 shown.
[0063] Test Example 2
[0064] As in Example 3, Mn 0.5 Co 2.5 O4 and Ce 0.5 Ti 0.5 O2 was loaded with 7:3, recorded as 70% Mn 0.5 Co 2.5 O4 / 30%Ce 0.5 Ti 0.5O2; the catalyst was placed in a fixed bed reactor and stability tested at 1% methane concentration; the temperature was programmed from 0 to 500°C, the reaction raw gas ratio was 1% methane, 20% O2, and the rest was Ar, the space velocity was 45000mL / (gh), and the methane conversion rate was observed; 100ppm SO2 was introduced on the basis of the raw gas, and the change in methane conversion rate was observed. The results are as follows Figure 3 shown.
[0065] Test Example 3
[0066] As in Example 4, Mn 0.5 Co 2.5 O4 and Ce 0.5 Ti 0.5 O2 was loaded with 8:2, recorded as 80% Mn 0.5 Co 2.5 O4 / 20%Ce 0.5 Ti 0.5 O2; the catalyst was placed in a fixed bed reactor and stability tested at a methane concentration of 1.5%; the temperature was programmed from 0 to 500°C, the reaction raw gas ratio was 1.5% methane, 20% O2, and the rest was Ar, the space velocity was 45000mL / (gh), and the methane conversion rate was observed; 100ppm SO2 was introduced on the basis of the raw gas, and the change in methane conversion rate was observed. The results are as follows Figure 4 shown.
[0067] As attached Figure 2-4 As shown, 100 ppm SO2 was introduced into the feed gas to study the sulfur resistance of different loading ratios in a fixed bed reactor. The catalysts all showed good sulfur resistance, and the catalytic activity in a sulfur-containing atmosphere was almost the same as that in a sulfur-free atmosphere, indicating that the stacking structure constructed by loading the Mn-Co-based solid solution catalyst on Ti-doped CeO2 and the two SO2 strong affinity sites formed by Ti-induced CeO2 crystal reconstruction improved the sulfur resistance of the catalyst.
[0068] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a methane combustion catalyst with high stability, characterized in that: The following steps are involved: (1) Preparation of Ce-Ti oxide by coprecipitation method C 12 H 28 O4Ti was dissolved in ethanol, and then Ce(NO3)3·6H2O was added to the solution and stirred for reaction. Then, the pH was adjusted with ammonia water, and the mixture was stirred for 2-4 hours. After aging for 2-4 hours, the precipitate was filtered and washed with water. The washed precipitate was dried and then heated in flowing air to obtain nanostructured Ce. x Ti 1-x O2 carrier, i.e. Ce-Ti oxide, Ce x Ti 1-x O2 where x = 0.1-0.9; (2) Loading Mn-Co solid solution on Ce-Ti oxide (2.1) Loading Mn-Co solid solution on Ce-Ti oxide by positive drop method Co(NO3)2·6H2O and Mn(CH3COO)2·4H2O are dissolved in water, which is referred to as solution A. Ce-Ti oxide and ammonium bicarbonate solution are then mixed, which is referred to as solution B. Solution A is slowly dripped into solution B, and after stirring for 1-8 hours, the mixture is filtered, and the precipitate is washed with ethanol and deionized water to a pH of 7-7.5 to obtain a sample. The sample is dried and calcined, urea is added to grind the sample, and the sample is calcined again to obtain a supported X Mn x Co 3-x O4 / Y Ce x Ti 1-x O2 catalyst; (2.2) Loading Mn-Co solid solution on Ce-Ti oxide by back-drip method Dissolve Co(NO3)2·6H2O, Mn(CH3COO)2·4H2O, and Ce-Ti oxide in water, then slowly drop ammonium bicarbonate solution, precipitate, stir, react, and age for 6-8h, filter, wash with ethanol and deionized water, and precipitate to pH 7-7.5 to obtain a sample. After drying, calcine the sample, add urea to grind, and calcine again to obtain supported X Mn x Co 3-x O4 / Y Ce x Ti 1-x O2 catalyst; Load type X Mn x Co 3-x O4 / Y Ce x Ti 1-x O2 catalyst formula: X:Y = 5-8:2-5, Mn x Co 1-x In O4, x = 0.1-3, Ce x Ti 1-x In O2, x=0.1-0.
9.
2. The method for preparing a methane combustion catalyst with high stability according to claim 1, characterized in that: The stirring reaction temperature in step (1) is 60-80° C., and the stirring reaction time is 20-40 min.
3. The method for preparing a methane combustion catalyst with high stability according to claim 1, characterized in that: The mass concentration of the ammonia water in step (1) is 6%, and the ammonia water is dripped into the solution at a dripping rate of 5 mL / min to adjust the pH to 8.5-10.
4. The method for preparing a methane combustion catalyst with high stability according to claim 1, characterized in that: The drying temperature in step (1) is 80-100° C. and the drying time is 10-12 h; The flowing air heating temperature is 400-500° C., the heating time is 3-4 hours, and the air flow rate is 20-50 ml / min.
5. The method for preparing a methane combustion catalyst with high stability according to claim 1, characterized in that: The dropping temperature in step (2.1) is 50-80°C, and the dropping speed is 5 ml / min; The concentration of the ammonium bicarbonate solution is 1 mol / L.
6. The method for preparing a methane combustion catalyst with high stability according to claim 1, characterized in that: The sample drying temperature in step (2.1) is 80-100°C and the drying time is 6-7h; The sample calcination temperature is 400-500°C and the calcination time is 3-4h; The mass ratio of the sample to urea is 1:4; The re-calcination temperature is 400-600° C., and the calcination time is 3-4 hours.
7. The method for preparing a methane combustion catalyst with high stability according to claim 1, characterized in that: The dropping temperature in step (2.2) is 60-70°C and the dropping speed is 5 ml / min; The concentration of the ammonium bicarbonate solution is 1 mol / L.
8. The method for preparing a methane combustion catalyst with high stability according to claim 1, characterized in that: The sample drying temperature in step (2.2) is 80-100°C and the drying time is 6-7h; The sample calcination temperature is 400-500°C and the calcination time is 3-4h; The mass ratio of the sample to urea is 1:4; The re-calcination temperature is 400-600° C., and the calcination time is 3-4 hours.
9. A methane combustion catalyst with high stability, characterized in that: The preparation method is described in any one of claims 1 to 8.
Citation Information
Patent Citations
Cobalt-manganese-cerium-bases titania catalyst and preparation method thereof
CN107999088A
Preparation method of manganese cerium catalyst with high catalytic activity in methane combustion and product
CN109701547A
Preparation method of Ce-Mn-Co-O oxygen carrier and application of Ce-Mn-Co-O oxygen carrier in hydrogen production by chemical-looping reforming of blast furnace gas
CN110844944A
Cobalt-cerium-manganese composite oxide catalyst for hydrogen production by autothermal reforming of acetic acid
CN111450840A
Preparation method and application of oxygen vacancy-enriched cerium oxide with echelon structure
CN117049586A
Cited By
ZrO2-MOx-coated SiO2 composite oxide, preparation method thereof and application of ZrO2-MOx-coated SiO2 composite oxide in catalytic oxidation of methane
CN120325269A