Method for obtaining phosphate concentrate and preparing high-strength gypsum by leaching low-grade phosphorite with organic acid
The calcium carbonate in low-grade phosphate rock is decomposed by low-concentration organic acid to obtain high-grade phosphate concentrate, and high-strength gypsum is prepared by recycling organic acid and hydrothermal method, which solves the problem of phosphogypsum storage and environmental pollution. , achieving economical, environmentally friendly and efficient utilization of phosphorus resources.
Patent Information
- Application Number
- CN202310384716.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-18
AI Technical Summary
Calcium resources in low-grade phosphate rocks cannot be effectively utilized, resulting in the accumulation of phosphogypsum occupying land and polluting the environment. In addition, the traditional flotation process has problems of high economic cost and low efficiency.
Use low-concentration organic acids to selectively decompose calcium carbonates in low-grade phosphate ores, obtain phosphate concentrates through solid-liquid separation, recycle organic acids in decalcification waste liquid, and prepare high-strength gypsum by combining hydrothermal methods. .
It achieves efficient enrichment of phosphate concentrate and preparation of high-strength gypsum, solves the problem of phosphogypsum occupying land and polluting the environment, reduces production costs, has economic and environmental significance, and promotes the sustainable development of the phosphorus resource industry.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical production, and in particular relates to a method for obtaining phosphate concentrate by leaching low-grade phosphate ore with organic acid and preparing high-strength gypsum. Background Art
[0002] Low-grade phosphate ore contains a large amount of calcium resources (30%-45%), which are discharged as industrial waste - phosphogypsum in the process of producing phosphoric acid by the traditional wet process - sulfuric acid process. Large-scale storage of phosphogypsum occupies land and pollutes the environment. Efficient utilization of the associated calcium resources in low-grade phosphate ore can solve the phosphogypsum problem from the source.
[0003] At present, high-strength gypsum has gradually replaced traditional building materials and applied in various fields due to its advantages of energy saving, good fire resistance and fast setting speed. Converting the associated calcium resources in low-grade phosphate ore into high-strength gypsum has high economic and social benefits.
[0004] Low-grade phosphate ore with high calcium carbonate content has poor compatibility with current flotation processes. When the ore contains crystalline carbonate, flotation technology can still achieve good results, but when the ore contains soft and chalky carbonate, it cannot achieve good flotation results; when carbonate crystals exist in the ore matrix in a symbiotic form, they must be finely crushed before they can be used for flotation separation of phosphorus; in addition, calcium carbonate has a greater impact on flotation due to its similar chemical behavior with phosphate. Calcination beneficiation can decompose calcium carbonate, but it requires a lot of heat to achieve the degree of beneficiation, and the economic cost is high.
[0005] Organic acids can selectively decompose carbonate minerals in phosphate ore at lower concentrations without affecting phosphates, and can play a role in enriching phosphorus. In this regard, Zhang Jie and others from Guizhou University have conducted relevant research and disclosed "A method for enriching low-grade phosphate ore using low-molecular weight organic acids" (CN108751150A). This method can enrich low-grade calcium-magnesium phosphate ore into phosphate concentrate ore with a P2O5 content greater than 35%, but does not consider the recovery of organic acids, resulting in high economic costs; Zhang Huali from Wuhan University of Technology has conducted relevant research on the use of organic acids to remove associated mineral resources and efficient utilization technology, and disclosed "A method for demagnesizing phosphate ore and preparing flame retardants using organic acids". This method obtains flame retardant products by leaching phosphate ore with organic acids, and also faces the problem of organic acid recovery and cost. In addition, the magnesium content in low-grade phosphate ore is usually lower than that of silicon and calcium, and the problem of comprehensive utilization of low-grade phosphate ore has not yet been solved. The present invention adopts organic acid to selectively decompose calcium carbonate in low-grade phosphate ore, and the obtained phosphate concentrate can directly enter the flotation process. The organic acid can be recycled through solid-liquid separation with a high-strength gypsum precursor. The high-strength gypsum is prepared from the high-strength gypsum under hydrothermal conditions, which has both economic and environmental significance and plays an important role in promoting the sustainable development of the phosphorus resource industry. Summary of the invention
[0006] The object of the present invention is to provide a method for obtaining phosphate concentrate and preparing high-strength gypsum by leaching low-grade phosphate ore with organic acid, and the method is specifically as follows:
[0007] (1) mixing low-grade phosphate ore with an organic acid solution to achieve a decalcification reaction of medium- and low-grade phosphate ore, and then obtaining decalcified waste liquid and phosphate concentrate through solid-liquid separation; (2) adding sulfuric acid to the decalcified waste liquid obtained in step (1), filtering to obtain a high-strength gypsum precursor and an organic acid solution; (3) mixing the high-strength gypsum precursor obtained in step (2) with a crystal medium and an activator, and performing a hydrothermal reaction at normal pressure; (4) after step (3) is completed, quickly washing, filtering, and drying to obtain a high-strength gypsum powder.
[0008] According to the above scheme, the low-grade phosphate ore in step (1) contains 12wt.%-20wt.% of P2O5, 33wt.%-45wt.% of calcium, and has a fineness of 100-200 mesh; the obtained phosphate concentrate contains 28 wt.%-38 wt.% of P2O5.
[0009] According to the above scheme, the organic acid in step (1) is any one of formic acid, acetic acid, and lactic acid, or a mixture of multiple thereof, and the organic acid concentration is 4%-10%.
[0010] According to the above scheme, the liquid-to-solid ratio in step (1) is (2:1)-(9:1); the temperature of the decalcification reaction is 40°C-75°C, and the decalcification reaction time is 20min-60min.
[0011] According to the above scheme, the concentration of sulfuric acid in step (2) is 0.5-2 mol / L, sulfuric acid is added at a uniform speed within 2 min-15 min, the temperature is 40°C-70°C, and the time is 150 min-300 min.
[0012] According to the above scheme, a control agent needs to be added in step (2). The function of the control agent is mainly to adjust the properties of the high-strength gypsum precursor. The control agent is mainly any one of aluminum chloride, ferric chloride, and sodium sulfate, or a mixture of multiple thereof. The concentration of the control agent is controlled to be 0.003 mol / L-0.05 mol / L.
[0013] According to the above scheme, the organic acid solution in step (2) can be reused through the circulation system.
[0014] According to the above scheme, the activator in step (3) is mainly a mixture of one or more of sodium sulfate, magnesium chloride, and calcium chloride, and the mass percentage concentration of the activator is 15%-40%; the crystallization medium is mainly a mixture of one or more of ammonium sulfate, potassium sulfate, sodium oxalate, and potassium tartrate, and the addition amount is 0.05%-0.5% of the mass of the high-strength gypsum precursor.
[0015] According to the above scheme, in step (3), the hydrothermal reaction is carried out at normal pressure, the liquid-to-solid ratio is (3:1)-(6:1), the temperature is 87-100°C, the pH value is 1-4, the stirring speed is 120rpm-250rpm, and the time is 4-10h.
[0016] According to the above scheme, the water temperature used for washing in step (4) is 75-90°C, the time is 10min-30min; the drying temperature is 55°C-105°C; and the purity of the obtained high-strength gypsum is 92%-99.5%.
[0017] The present invention selectively decomposes calcium carbonate in low-grade phosphate rock powder (100 mesh-200 mesh), and obtains phosphate concentrate with a P2O5 content of 28 wt.%-38 wt.% through solid-liquid separation; high-strength gypsum precursor and organic acid solution can be obtained by adding sulfuric acid and filtering, and the organic acid solution can enter a circulation system for reuse; the high-strength gypsum is prepared from the high-strength gypsum precursor under hydrothermal conditions, and high-purity high-strength gypsum with a purity of 92%-99.5% and an absolute dry compressive strength of 35MPa-80MPa is obtained by controlling process parameters such as the amount of an activator, the amount of a crystal mediator, the liquid-solid ratio, the temperature, the pH value, and the stirring speed.
[0018] In the present invention, in step (1), the fineness of low-grade phosphate ore, organic acid concentration, liquid-to-solid ratio, reaction temperature and reaction time are controlled in order to obtain high-grade phosphate concentrate; in step (2), the sulfuric acid concentration, control agent dosage, reaction time and temperature are controlled in order to obtain a pure organic acid solution and a high-quality high-strength gypsum precursor; in step (3), the amount of activator, the amount of crystal mediator, liquid-to-solid ratio, temperature, pH value, stirring speed and other process parameters are controlled in order to regulate the crystal growth rate and obtain high-purity and high-strength high-strength gypsum; in step (4), the temperature of washing water, washing time and drying temperature are controlled in order to obtain high-purity high-strength gypsum powder.
[0019] The beneficial effects of the present invention are as follows: (1) The present invention utilizes organic acid to leach low-grade phosphate ore to obtain phosphate concentrate with a P2O5 content of 28 wt.%-38 wt.%, and solves the influence of soft and chalky calcium carbonate on flotation, and can directly enter the flotation process. (2) The present invention uses decalcified waste liquid to prepare a high-strength gypsum precursor, realizes the recycling of organic acid, and has extremely high economic value. (3) The present invention uses a normal pressure hydrothermal method to prepare a high-strength gypsum from a high-strength gypsum precursor, which can be used in many fields of the building materials industry and has high added value; and solves the problem of phosphogypsum occupying land and polluting the environment from the source, and has extremely high economic and social benefits. DETAILED DESCRIPTION
[0020] The invention of this application is further described below in conjunction with examples, but the examples should not be regarded as limiting the rights of the present invention.
[0021] Embodiment 1:
[0022] The chemical composition of a low-grade phosphate rock is: P2O5 18.35%, CaCO3 35.59%, SiO2 16.92%.
[0023] A method for leaching low-grade phosphate ore with organic acid to obtain phosphate concentrate and prepare high-strength gypsum, comprising the following steps:
[0024] (1) Grind the phosphate rock to 200 mesh for later use. Weigh 120g of 7% formic acid solution and place it in a 500mL flask. Heat it to 50°C in a water bath. Weigh 20g of phosphate rock powder. When the temperature of the formic acid solution rises to 50°C, gradually add the phosphate rock powder into the three-necked flask and stir. After reacting for 50 minutes, filter to obtain decalcified waste liquid and phosphate concentrate. Wash the phosphate concentrate three times, using 30mL of distilled water each time. The washing water can be directly added to the decalcified waste liquid.
[0025] (2) Add 350 mL of 0.5 mol / L sulfuric acid solution to the decalcified waste liquid obtained in step (1) at a uniform rate within 3 minutes, and add 0.45 g of ferric chloride. At 65°C, react for 180 minutes and then filter to obtain an organic acid solution and a high-strength gypsum precursor. The organic acid solution enters the circulation system and is reused.
[0026] (3) Select (2 / 3Na2SO4+1 / 3MgCl2) as the activator, prepare 200 mL of a 25% activator solution in a 500 mL three-necked flask, and place it in a 90°C water bath. Weigh 100 g of dried high-strength gypsum precursor and 0.08 g of potassium tartrate, and gradually add the activator solution to the three-necked flask after the temperature rises to 90°C. Turn on the stirring, control the stirring rate to 150 rpm, and the pH to 2.
[0027] (4) After reacting for 8 hours, wash with 85°C hot water for 15 minutes and dry at 90°C to constant weight to obtain high-strength gypsum powder.
[0028] The P2O5 content in the phosphate concentrate obtained in step (1) was determined by the quinoline phosphomolybdic acid weight method. The results showed that the P2O5 content in the phosphate concentrate increased to 30.32%.
[0029] The high-strength gypsum powder obtained in step (4) was tested for performance, and the results showed that the purity was 96.8% and the absolute dry compressive strength was 52.3 MPa.
[0030] Embodiment 2:
[0031] The chemical composition of a low-grade phosphate rock is: P2O5 19.61%, CaCO3 40.29%, SiO2 4.379%.
[0032] A method for leaching low-grade phosphate ore with organic acid to obtain phosphate concentrate and prepare high-strength gypsum, comprising the following steps:
[0033] (1) Grind the phosphate rock to 200 mesh for later use. Weigh 160g of 6% lactic acid solution and place it in a 500mL flask. Heat it to 50°C in a water bath. Weigh 20g of phosphate rock powder and wait until the temperature of the formic acid solution rises to 65°C. Gradually add the phosphate rock powder to the three-necked flask and stir. After reacting for 50 minutes, filter to obtain decalcified waste liquid and phosphate concentrate. Wash the phosphate concentrate three times, using 30mL of distilled water each time. The washing water can be directly added to the decalcified waste liquid.
[0034] (2) Add 280 mL of 0.7 mol / L sulfuric acid solution to the decalcified waste liquid obtained in step (1) at a uniform rate within 3 minutes, and add 0.8 g of ferric chloride. At 60°C, react for 210 minutes and filter to obtain an organic acid solution and a high-strength gypsum precursor. The organic acid solution enters the circulation system and is reused.
[0035] (3) Select (2 / 3CaCl2+1 / 3MgCl2) as the activator, prepare 200 mL of a 34% activator solution in a 500 mL three-necked flask, and place it in a 90°C water bath. Weigh 100 g of dried high-strength gypsum precursor and 0.1 g of sodium oxalate, and gradually add the activator solution to the three-necked flask after the temperature rises to 90°C. Turn on the stirring, control the stirring rate to 150 rpm, and the pH to 1.8.
[0036] (4) After reacting for 8 hours, wash with 85°C hot water for 15 minutes and dry at 90°C to constant weight to obtain high-strength gypsum powder.
[0037] The P2O5 content in the phosphate concentrate obtained in step (1) was determined by the quinoline phosphomolybdic acid weight method. The results showed that the P2O5 content in the phosphate concentrate increased to 33.32%.
[0038] The high-strength gypsum powder obtained in step (4) was tested for performance, and the results showed that the purity was 97.3% and the absolute dry compressive strength was 65.9 MPa.
Claims
1. A method for leaching low-grade phosphate ore using organic acid to obtain phosphate concentrate and prepare high-strength gypsum, characterized in that: Including the following process: (1) Mixing low-grade phosphate ore with an organic acid solution to achieve a decalcification reaction of the low-grade phosphate ore, and then obtaining decalcified waste liquid and phosphate concentrate through solid-liquid separation; (2) adding sulfuric acid to the decalcified waste liquid obtained in step (1), and filtering to obtain a high-strength gypsum precursor and an organic acid solution; (3) mixing the high-strength gypsum precursor obtained in step (2) with a crystal medium and an activator, and performing a hydrothermal reaction at normal pressure; (4) After step (3) is completed, the high-strength gypsum powder is quickly washed, filtered and dried.
2. The method of obtaining phosphate concentrate and preparing high-strength gypsum by leaching low-grade phosphate ore with organic acid according to claim 1, characterized in that: In step (1), the low-grade phosphate ore contains 12wt.%-20wt.% of P2O5, 33wt.%-45wt.% of calcium, and has a fineness of 100-200 mesh; the obtained phosphate concentrate contains 28wt.%-38wt.% of P2O5.
3. The method of obtaining phosphate concentrate and preparing high-strength gypsum by leaching low-grade phosphate ore with organic acid according to claim 1, characterized in that: In step (1), the organic acid is any one of formic acid, acetic acid and lactic acid or a mixture of multiple thereof, and the mass percentage concentration of the organic acid is 4%-10%.
4. The method of obtaining phosphate concentrate and preparing high-strength gypsum by leaching low-grade phosphate ore with organic acid according to claim 1, characterized in that: In step (1), the liquid-to-solid ratio is (2:1)-(9:1); the decalcification reaction temperature is 40°C-75°C, and the decalcification reaction time is 20min-60min.
5. The method of obtaining phosphate concentrate and preparing high-strength gypsum by leaching low-grade phosphate ore with organic acid according to claim 1, characterized in that: In step (2), the concentration of sulfuric acid is 0.5-2 mol / L, and sulfuric acid is added at a uniform speed within 2 min-15 min, the temperature is 40°C-70°C, and the time is 150 min-300 min.
6. The method of claim 1 for obtaining phosphate concentrate by leaching low-grade phosphate ore with organic acid and preparing high-strength gypsum, characterized in that: In step (2), a control agent is also added. The main function of the control agent is to adjust the properties of the high-strength gypsum precursor. The control agent is mainly any one of aluminum chloride, ferric chloride, and sodium sulfate, or a mixture of multiple thereof, with an addition amount of 0.05 mol / L-0.3 mol / L.
7. The method of claim 1 for obtaining phosphate concentrate by leaching low-grade phosphate ore with organic acid and preparing high-strength gypsum, characterized in that: The organic acid solution in step (2) can be reused after passing through the circulation system.
8. The method of obtaining phosphate concentrate and preparing high-strength gypsum by leaching low-grade phosphate ore with organic acid according to claim 1, characterized in that: In step (3), the activator is mainly a mixture of one or more of sodium sulfate, magnesium chloride, and calcium chloride, and the mass percentage concentration of the activator is 15%-40%; the crystallizing agent is mainly a mixture of one or more of ammonium sulfate, potassium sulfate, sodium oxalate, and potassium tartrate, and the addition amount is 0.05%-0.5% of the high-strength gypsum precursor.
9. The method of claim 1 for obtaining phosphate concentrate by leaching low-grade phosphate ore with organic acid and preparing high-strength gypsum, characterized in that: In step (3), the hydrothermal reaction is carried out at normal pressure, with a liquid-to-solid ratio of (3:1) to (6:1), a temperature of 87 to 100°C, a pH value of 1 to 4, a stirring speed of 120 rpm to 250 rpm, and a time of 4 to 10 hours.
10. The method of obtaining phosphate concentrate and preparing high-strength gypsum by leaching low-grade phosphate ore with organic acid according to claim 1, characterized in that: In step (4), the temperature of the water used for washing is 75-90°C, and the time is 10 min-30 min; the drying temperature is 55°C-105°C, and the purity of the obtained high-strength gypsum is 92%-99.5%.
Citation Information
Cited By
Method for recycling valuable elements in phosphorite step by step through gradient acid leaching
CN121183119A