High-strength corrosion-resistant aluminum-silicon glass and preparation method thereof
Through the modification technology of silane monomer and graphene oxide, a fluorinated layer is formed, which solves the corrosion problem of aluminosilicate glass in acid and alkali environments, significantly improves its corrosion resistance and hydrophobicity, and extends its service life.
Patent Information
- Application Number
- CN202411062538.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-02
AI Technical Summary
Aluminosilicate glass is easily corroded in acid and alkali environments, resulting in reduced optical performance, weakened mechanical strength and shortened service life. It is difficult to effectively improve its corrosion resistance with existing technology.
Mercaptochloropropylpolysiloxane was prepared by using silane monomers such as octamethylcyclotetrasiloxane, γ-chloropropylmethyldiethoxysilane, and γ-mercaptopropyltriethoxysilane, and Substitution and quaternization reaction of sodium iodide and triethylamine, Formation of mercapto quaternary ammonium salt polysiloxane, followed by ion replacement and modification with graphene oxide, combined with the POSS structure to form a fluorinated layer, improves the dispersion and compactness of the coating liquid, and forms a coating with physical barrier and super hydrophobicity layer.
It significantly improves the corrosion resistance of aluminosilicate glass, prevents the intrusion of water and corrosive media, avoids the occurrence of cracks, and enhances its resistance to alkali corrosion through the microporous/mesoporous combined structure formed by the fluorinated layer.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminosilicate glass, and in particular to high-strength corrosion-resistant aluminosilicate glass and a preparation method thereof. Background Art
[0002] Aluminosilicate glass is a material with excellent physical and chemical properties. It is widely used in electronic information product covers, aviation transparent devices, and observation windows for ships, special vehicles, and deep-sea detectors. This type of glass is favored for its low thermal expansion coefficient and good mechanical properties, especially in high temperature or extreme environments. However, aluminosilicate glass is susceptible to corrosion in acidic and alkaline environments, especially glass containing high concentrations of alkali metal ions (such as Li+), where the corrosion phenomenon is more significant. This corrosion usually manifests itself as haziness, powdering, and the appearance of corrosion pits on the surface, which not only seriously affects the optical properties and appearance of the glass, but may also cause a decrease in the mechanical strength of the material, affecting its service life and safety.
[0003] The corrosion mechanism of aluminosilicate glass is mainly caused by the ion exchange between H+ or OH- and alkali metal ions (such as Na+, K+) in the glass. When the glass is exposed to water or an acidic environment, the H+ or H3O+ in the solution will penetrate into the glass structure and exchange with the alkali metal ions to form Si-OH groups. These groups will further hydrolyze, destroying the Si-O-Si bond, generating non-bridging oxygen Si-OH, and finally forming silicic acid and OH-. In an alkaline environment, OH- attacks the Si-O bond on the surface of the glass, causing the silicon-oxygen network structure to be destroyed and generating silicate ions. These ions combine with the cations on the surface of the glass to form silicates, which eventually dissolve in the alkaline solution.
[0004] Due to the corrosion problem of aluminosilicate glass, researchers have proposed a variety of methods to improve its corrosion resistance. A common method is to add anti-corrosion additives during the glass forming process, which can significantly improve the glass's resistance to chemical erosion. For example, by adding certain oxides or fluorides, the stability of the glass network can be enhanced, thereby reducing the occurrence of corrosion. Another method is to coat the glass surface to form a protective coating to isolate it from contact with corrosive media. For example, coating a layer of MgF2 protective film on a phosphate glass filter can effectively improve its corrosion resistance in tropical marine environments.
[0005] In addition, the corrosion resistance of glass can also be improved by optimizing its chemical composition. For example, reducing the content of alkali metal and alkaline earth metal ions in glass, or increasing the content of SiO2, can help enhance the chemical stability of glass. Studies have shown that the higher the SiO2 content in glass, the more stable its structure and the stronger its resistance to acid and alkali media. On the other hand, improving the density and uniformity of glass and reducing the presence of internal defects and microcracks can also help improve its corrosion resistance.
[0006] Therefore, it is of great significance to invent a high-strength corrosion-resistant aluminosilicate glass. Summary of the invention
[0007] The object of the present invention is to provide a high-strength corrosion-resistant aluminosilicate glass and a preparation method thereof to solve the problems raised in the above-mentioned background technology.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0009] A method for preparing high-strength corrosion-resistant aluminosilicate glass comprises the following steps:
[0010] S1: ultrasonically treat the LAS glass in ethanol, acetone, and deionized water for 15-30 min in sequence and set aside;
[0011] Step (1): octamethylcyclotetrasiloxane, γ-chloropropylmethyldiethoxysilane and γ-mercaptopropyltriethoxysilane are added to a reaction vessel and stirred evenly, concentrated sulfuric acid is added, and the mixture is heated to 60-65° C. and reacted for 6-8 hours. Extraction is performed with deionized water and dichloromethane, and the process is repeated three times. The aqueous phase is removed, and the organic phase is heated to 40-45° C. and the solvent is removed by rotary evaporation to obtain mercaptochloropropyl polysiloxane;
[0012] Furthermore, in the mercaptochloropropyl polysiloxane, the molar ratio of octamethylcyclotetrasiloxane:γ-chloropropylmethyldiethoxysilane:γ-mercaptopropyltriethoxysilane:concentrated sulfuric acid is 3.5:(2-4):(1-3):3.5;
[0013] Step (2): adding sodium iodide to acetone and stirring evenly, adding mercaptochloropropyl polysiloxane, heating to 70-75°C and reflux reaction for 48-50h, filtering, heating the filtrate to 60-65°C and rotary evaporating to remove the solvent, extracting the residue with ether, heating to 35-37°C and rotary evaporating to remove the ether, and obtaining mercaptoiodopropyl polysiloxane;
[0014] Furthermore, in the mercaptoiodopropyl polysiloxane, the mass ratio of mercaptochloropropyl polysiloxane to sodium iodide is 4:(0.8-1);
[0015] Step (3): adding mercapto iodopropyl polysiloxane to tetrahydrofuran, adding triethylamine, heating to 40-45° C. and stirring to react for 72-74 hours, heating to 60-65° C. and rotary evaporating to remove the solvent, washing with ethanol, and drying at 60-65° C. to obtain mercapto quaternary ammonium salt polysiloxane;
[0016] Furthermore, in the mercapto quaternary ammonium salt polysiloxane, the mass ratio of mercapto iodopropyl polysiloxane to triethylamine is 9:(4-5);
[0017] S2: ultrasonically dispersing graphene oxide in deionized water, adding 0.1 M sodium hydroxide to adjust the pH to 7.5-8, adding a chloroform solution of mercapto quaternary ammonium salt polysiloxane, and ultrasonically dispersing for 30-45 minutes to obtain modified graphene oxide;
[0018] Furthermore, in the modified graphene oxide, the mass ratio of graphene oxide to mercapto quaternary ammonium salt polysiloxane is 0.002 to (0.15-0.3);
[0019] S3: adding modified graphene oxide to a dichloromethane solution of 8-methacrylic acid POSS and 0.15-0.2wt% 2-hydroxy-2-methylacetophenone, irradiating with ultraviolet light for 40-45min, washing with ethanol, and drying at 60-65°C to obtain POSS-modified graphene oxide; adding POSS-modified graphene oxide and azobisisobutyronitrile to HFO, heating to 85-87°C under a nitrogen atmosphere, adding 2-(perfluorooctyl)ethyl methacrylate, azobisisobutyronitrile, and HFO, keeping the temperature for reaction for 1-2h, washing with ethanol, and drying at 60-65°C to obtain fluorinated POSS-modified graphene oxide;
[0020] Further, in the POSS-modified graphene oxide, the mass ratio of modified graphene oxide: 8-methylallyl POSS is 1: (40-50); in the fluorinated POSS-modified graphene oxide, the mass ratio of POSS-modified graphene oxide: 2-(perfluorooctyl)ethyl methacrylate is (0.15-0.2): (6-8);
[0021] Furthermore, the HFO is 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether.
[0022] S4: Ultrasonic dispersion of fluorinated POSS modified graphene oxide in deionized water to obtain graphene dispersion; adding tetraethyl orthosilicate into ethanol and stirring evenly, adding hydrochloric acid, heating to 30-31°C and stirring for 24h to obtain tetraethyl orthosilicate hydrolyzate; placing fluorinated POSS modified graphene oxide, graphene dispersion and tetraethyl orthosilicate hydrolyzate at 30-31°C and stirring for 7-8h to obtain coating solution;
[0023] Further, the concentration of the graphene dispersion is 0.003-0.005 g / mL; the concentration of the hydrochloric acid is 1.3 M; in the tetraethyl orthosilicate hydrolyzate, the volume ratio of tetraethyl orthosilicate: ethanol: hydrochloric acid is (3.5-3.75): 5: (1.25-1.5); in the coating solution, 15 mL of graphene dispersion and 10 mL of tetraethyl orthosilicate hydrolyzate are added to every 0.05 g of fluorinated POSS modified graphene oxide;
[0024] S5: Spin-coat the coating liquid on the surface of the LAS glass, heat it to 100-101°C in a nitrogen atmosphere and keep it for 1-1.5 hours, continue to heat it to 550-650°C and keep it for 2-2.5 hours, and cool it to room temperature to obtain high-strength corrosion-resistant aluminosilicate glass.
[0025] Furthermore, the coating solution has a thickness of 3-5 μm; and the heating rate during the heating process is 2° C. / min.
[0026] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0027] The invention uses octamethylcyclotetrasiloxane, γ-chloropropylmethyldiethoxysilane and γ-mercaptopropyltriethoxysilane as silane monomer raw materials to prepare linear polysilane containing mercapto and chloropropyl side chain structures, and then sequentially performs substitution and quaternization reactions on the linear polysilane with sodium iodide and triethylamine to prepare mercapto quaternary ammonium salt polysiloxane; finally, the linear polysilane is subjected to ion replacement with weakly alkaline treated graphene oxide, and the polysiloxane is grafted on the surface of the graphene oxide to prepare modified graphene oxide. On the one hand, the dispersibility of graphene oxide in the subsequent coating liquid component tetraethyl orthosilicate is improved to avoid the occurrence of agglomeration problems; on the other hand, the two-dimensional sheet structure of graphene is utilized to increase the penetration path of the corrosive medium and to seal the pores formed during the curing process of the coating layer, thereby playing a physical barrier role while also having excellent corrosion resistance, greatly improving the corrosion resistance of aluminosilicate glass; during the high-temperature curing process, linear polysiloxane and tetraethyl orthosilicate undergo dehydration and condensation and the network becomes densified. The network structure formed by Si-O-Si bonds can improve the hydrophobicity of aluminosilicate glass and effectively prevent the intrusion of water and corrosive media. The addition of tetraethyl orthosilicate can improve the integrity and density of the polysiloxane coating and avoid the appearance of cracks during the formation of the polysiloxane coating.
[0028] In order to further enhance the corrosion resistance of aluminosilicate glass, 8-methacrylic acid POSS was introduced into the modified graphene oxide structure by ultraviolet click chemistry reaction through the thiol group in the linear polysiloxane structure on the surface of modified graphene, and then polymerized with 2-(perfluorooctyl)ethyl methacrylate free radicals to obtain fluorinated POSS modified graphene oxide; due to the low surface energy characteristics of the long-chain fluorocarbon structure of the fluorinated POSS modified graphene oxide, the POSS structure will preferentially migrate to the surface of the coating layer during the curing process to form a rough structure of micropores / mesopores, which gives the aluminosilicate glass superhydrophobicity and cooperates with the surface fluorinated layer to achieve super-amphiphobic characteristics; the introduction of the POSS structure increases the interlayer spacing of graphene oxide due to the special cage structure, making the invasion path of the corrosive medium more tortuous; due to the alkali corrosion mechanism of glass, the outermost fluorinated layer can prevent the silica network structure of the film layer from frequent contact with the alkaline solution; the combined effect of the two further improves the corrosion resistance of the aluminosilicate glass. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] In the following examples, graphene oxide was purchased from Changzhou Sixth Element Materials Technology Co., Ltd.; the remaining raw materials were commercially available.
[0031] The LAS aluminosilicate glass components include, by mass percentage, 70.81% SiO2, 4.76% Al2O3, 0.80% P2O5, 1.62ZrO2, 1.39% MgO, 0.32% ZnO, 0.36% Na2O, 0.66% K2O, 19.08% Li2O,
[0032] 0.20% B2O3;
[0033] The preparation method includes adding glass raw materials into a mixed concentrate and mixing them evenly, introducing them into a platinum crucible, heating them to 1600°C to melt them for 6 hours, introducing the glass liquid into a mold to obtain glass bricks, placing the glass bricks in a 480°C annealing furnace to keep them warm for 48 hours, annealing them, and wire-cutting the annealed glass bricks to obtain LAS aluminosilicate glass sheets; the size is 50mm×50mm×0.8mm.
[0034] The preparation method of the mercapto quaternary ammonium salt polysiloxane comprises the following steps:
[0035] Step (1): 3.5 mol of octamethylcyclotetrasiloxane, 2 mol of γ-chloropropylmethyldiethoxysilane and 3 mol of γ-mercaptopropyltriethoxysilane are added to a reaction vessel and stirred evenly, 3.5 mol of concentrated sulfuric acid is added, the mixture is heated to 60° C. and reacted for 6 h, and deionized water and dichloromethane are extracted, and the process is repeated three times. The aqueous phase is removed, and the organic phase is heated to 40° C. and the solvent is removed by rotary evaporation to obtain mercaptochloropropyl polysiloxane;
[0036] Step (2): add 1 g of sodium iodide to acetone and stir evenly, add 4 g of mercaptochloropropyl polysiloxane, heat to 70° C. and reflux for 48 h, filter, heat the filtrate to 60° C. and evaporate to remove the solvent, extract the residue with ether, heat to 35° C. and evaporate to remove the ether, to obtain mercaptoiodopropyl polysiloxane;
[0037] Step (3): Add 9 g of mercapto iodopropyl polysiloxane to tetrahydrofuran, add 4 g of triethylamine, heat to 40° C. and stir to react for 72 h, heat to 60° C. and evaporate to remove the solvent, wash with ethanol, and dry at 60° C. to obtain mercapto quaternary ammonium salt polysiloxane.
[0038] Example 1: A method for preparing high-strength corrosion-resistant aluminosilicate glass: S1: ultrasonically disperse 0.002 g of graphene oxide in deionized water, add 0.1 M sodium hydroxide to adjust the pH to 7.5, add 0.15 g of chloroform solution of mercapto quaternary ammonium salt polysiloxane, and ultrasonically disperse for 30-45 min to obtain modified graphene oxide;
[0039] S2: 1 g of modified graphene oxide was added to a dichloromethane solution of 4098-methacrylic acid POSS and 0.15 wt% 2-hydroxy-2-methylacetophenone, irradiated with ultraviolet light for 40 min, washed with ethanol, and dried at 60 ° C to obtain POSS modified graphene oxide; 0.15 g of POSS modified graphene oxide and azobisisobutyronitrile were added to HFO, heated to 85 ° C under a nitrogen atmosphere, 692-(perfluorooctyl)ethyl methacrylate, azobisisobutyronitrile, and HFO mixture were added, and the reaction was kept warm for 1 h, washed with ethanol, and dried at 60 ° C to obtain fluorinated POSS modified graphene oxide;
[0040] S3: Ultrasonic dispersion of 0.03 g of fluorinated POSS modified graphene oxide in deionized water to obtain a graphene dispersion with a concentration of 0.003 g / mL; 3.5 mL of tetraethyl orthosilicate was added to 5 mL of ethanol and stirred evenly, 1.5 mL of hydrochloric acid was added, and the mixture was heated to 30°C and stirred for 24 h to obtain a tetraethyl orthosilicate hydrolyzate; 0.05 g of fluorinated POSS modified graphene oxide, 15 mL of graphene dispersion, and 10 mL of tetraethyl orthosilicate hydrolyzate were placed at 30°C and stirred for 7 h to obtain a coating solution;
[0041] S4: The LAS glass was ultrasonically treated in ethanol, acetone, and deionized water for 15 min in sequence for later use;
[0042] S5: Spin-coat the coating liquid on the surface of LAS glass, heat to 100°C at a heating rate of 2°C / min in a nitrogen atmosphere and keep it warm for 1 hour, continue to heat to 600°C at a heating rate of 2°C / min and keep it warm for 2 hours, cool to room temperature, and obtain high-strength corrosion-resistant aluminosilicate glass; the coating liquid thickness is 5μm.
[0043] Example 2: A method for preparing high-strength, corrosion-resistant aluminosilicate glass: S1: ultrasonically disperse 0.002 g of graphene oxide in deionized water, add 0.1 M sodium hydroxide to adjust the pH to 7.5, add 0.3 g of a chloroform solution of a mercapto quaternary ammonium salt polysiloxane, and ultrasonically disperse for 30-45 min to obtain modified graphene oxide;
[0044] S2: 1 g of modified graphene oxide was added to a dichloromethane solution of 4098-methacrylic acid POSS and 0.15 wt% 2-hydroxy-2-methylacetophenone, irradiated with ultraviolet light for 40 min, washed with ethanol, and dried at 60 ° C to obtain POSS modified graphene oxide; 0.15 g of POSS modified graphene oxide and azobisisobutyronitrile were added to HFO, heated to 85 ° C under a nitrogen atmosphere, 692-(perfluorooctyl)ethyl methacrylate, azobisisobutyronitrile, and HFO mixture were added, and the reaction was kept warm for 1 h, washed with ethanol, and dried at 60 ° C to obtain fluorinated POSS modified graphene oxide;
[0045] S3: Ultrasonic dispersion of 0.03 g of fluorinated POSS modified graphene oxide in deionized water to obtain a graphene dispersion with a concentration of 0.003 g / mL; 3.5 mL of tetraethyl orthosilicate was added to 5 mL of ethanol and stirred evenly, 1.5 mL of hydrochloric acid was added, and the mixture was heated to 30°C and stirred for 24 h to obtain a tetraethyl orthosilicate hydrolyzate; 0.05 g of fluorinated POSS modified graphene oxide, 15 mL of graphene dispersion, and 10 mL of tetraethyl orthosilicate hydrolyzate were placed at 30°C and stirred for 7 h to obtain a coating solution;
[0046] S4: The LAS glass was ultrasonically treated in ethanol, acetone, and deionized water for 15 min in sequence for later use;
[0047] S5: Spin-coat the coating liquid on the surface of LAS glass, heat to 100°C at a heating rate of 2°C / min in a nitrogen atmosphere and keep it warm for 1 hour, continue to heat to 600°C at a heating rate of 2°C / min and keep it warm for 2 hours, cool to room temperature, and obtain high-strength corrosion-resistant aluminosilicate glass; the coating liquid thickness is 5μm.
[0048] Example 3: A method for preparing high-strength, corrosion-resistant aluminosilicate glass: S1: ultrasonically disperse 0.002 g of graphene oxide in deionized water, add 0.1 M sodium hydroxide to adjust the pH to 7.5, add 0.3 g of a chloroform solution of a mercapto quaternary ammonium salt polysiloxane, and ultrasonically disperse for 30-45 min to obtain modified graphene oxide;
[0049] S2: 1 g of modified graphene oxide was added to a dichloromethane solution of 4098-methacrylic acid POSS and 0.15 wt% 2-hydroxy-2-methylacetophenone, irradiated with a UV lamp for 40 min, washed with ethanol, and dried at 60 ° C to obtain POSS-modified graphene oxide; 0.2 g of POSS-modified graphene oxide and azobisisobutyronitrile were added to HFO, heated to 85 ° C under a nitrogen atmosphere, 892-(perfluorooctyl)ethyl methacrylate, azobisisobutyronitrile, and HFO mixture were added, and the reaction was kept warm for 1 h, washed with ethanol, and dried at 60 ° C to obtain fluorinated POSS-modified graphene oxide;
[0050] S3: Ultrasonic dispersion of 0.03 g of fluorinated POSS modified graphene oxide in deionized water to obtain a graphene dispersion with a concentration of 0.003 g / mL; 3.5 mL of tetraethyl orthosilicate was added to 5 mL of ethanol and stirred evenly, 1.5 mL of hydrochloric acid was added, and the mixture was heated to 30°C and stirred for 24 h to obtain a tetraethyl orthosilicate hydrolyzate; 0.05 g of fluorinated POSS modified graphene oxide, 15 mL of graphene dispersion, and 10 mL of tetraethyl orthosilicate hydrolyzate were placed at 30°C and stirred for 7 h to obtain a coating solution;
[0051] S4: The LAS glass was ultrasonically treated in ethanol, acetone, and deionized water for 15 min in sequence for later use;
[0052] S5: Spin-coat the coating liquid on the surface of LAS glass, heat to 100°C at a heating rate of 2°C / min in a nitrogen atmosphere and keep it warm for 1 hour, continue to heat to 600°C at a heating rate of 2°C / min and keep it warm for 2 hours, cool to room temperature, and obtain high-strength corrosion-resistant aluminosilicate glass; the coating liquid thickness is 5μm.
[0053] Example 4: A method for preparing high-strength, corrosion-resistant aluminosilicate glass: S1: ultrasonically disperse 0.002 g of graphene oxide in deionized water, add 0.1 M sodium hydroxide to adjust the pH to 7.5, add 0.3 g of a chloroform solution of a mercapto quaternary ammonium salt polysiloxane, and ultrasonically disperse for 30-45 min to obtain modified graphene oxide;
[0054] S2: 1 g of modified graphene oxide was added to a dichloromethane solution of 4098-methacrylic acid POSS and 0.15 wt% 2-hydroxy-2-methylacetophenone, irradiated with a UV lamp for 40 min, washed with ethanol, and dried at 60 ° C to obtain POSS-modified graphene oxide; 0.2 g of POSS-modified graphene oxide and azobisisobutyronitrile were added to HFO, heated to 85 ° C under a nitrogen atmosphere, 892-(perfluorooctyl)ethyl methacrylate, azobisisobutyronitrile, and HFO mixture were added, and the reaction was kept warm for 1 h, washed with ethanol, and dried at 60 ° C to obtain fluorinated POSS-modified graphene oxide;
[0055] S3: Ultrasonic dispersion of 0.05 g of fluorinated POSS modified graphene oxide in deionized water to obtain a graphene dispersion with a concentration of 0.005 g / mL; 3.5 mL of tetraethyl orthosilicate was added to 5 mL of ethanol and stirred evenly, 1.5 mL of hydrochloric acid was added, and the mixture was heated to 30°C and stirred for 24 h to obtain a tetraethyl orthosilicate hydrolyzate; 0.05 g of fluorinated POSS modified graphene oxide, 15 mL of graphene dispersion, and 10 mL of tetraethyl orthosilicate hydrolyzate were placed at 30°C and stirred for 7 h to obtain a coating solution;
[0056] S4: The LAS glass was ultrasonically treated in ethanol, acetone, and deionized water for 15 min in sequence for later use;
[0057] S5: Spin-coat the coating liquid on the surface of LAS glass, heat to 100°C at a heating rate of 2°C / min in a nitrogen atmosphere and keep it warm for 1 hour, continue to heat to 600°C at a heating rate of 2°C / min and keep it warm for 2 hours, cool to room temperature, and obtain high-strength corrosion-resistant aluminosilicate glass; the coating liquid thickness is 5μm.
[0058] Comparative Example 1: A method for preparing high-strength corrosion-resistant aluminosilicate glass: S1: ultrasonically disperse 0.002 g of graphene oxide in deionized water, add 0.1 M sodium hydroxide to adjust the pH to 7.5, add 0.15 g of chloroform solution of mercapto quaternary ammonium salt polysiloxane, and ultrasonically disperse for 30-45 min to obtain modified graphene oxide;
[0059] S2: 1 g of modified graphene oxide was added to a dichloromethane solution of 4098-methacrylic acid POSS and 0.15 wt% 2-hydroxy-2-methylacetophenone, irradiated with ultraviolet light for 40 min, washed with ethanol, and dried at 60 ° C to obtain POSS modified graphene oxide; 0.15 g of POSS modified graphene oxide and azobisisobutyronitrile were added to HFO, heated to 85 ° C under a nitrogen atmosphere, 692-(perfluorooctyl)ethyl methacrylate, azobisisobutyronitrile, and HFO mixture were added, and the reaction was kept warm for 1 h, washed with ethanol, and dried at 60 ° C to obtain fluorinated POSS modified graphene oxide;
[0060] S3: Ultrasonic dispersion of 0.03 g of fluorinated POSS modified graphene oxide in deionized water to obtain a graphene dispersion with a concentration of 0.003 g / mL; 1 mL of tetraethyl orthosilicate was added to 5 mL of ethanol and stirred evenly, 1.5 mL of hydrochloric acid was added, and the mixture was heated to 30°C and stirred for 24 h to obtain a tetraethyl orthosilicate hydrolyzate; 0.05 g of fluorinated POSS modified graphene oxide, 15 mL of graphene dispersion, and 10 mL of tetraethyl orthosilicate hydrolyzate were placed at 30°C and stirred for 7 h to obtain a coating solution;
[0061] S4: The LAS glass was ultrasonically treated in ethanol, acetone, and deionized water for 15 min in sequence for later use;
[0062] S5: Spin-coat the coating liquid on the surface of LAS glass, heat to 100°C at a heating rate of 2°C / min in a nitrogen atmosphere and keep it warm for 1 hour, continue to heat to 600°C at a heating rate of 2°C / min and keep it warm for 2 hours, cool to room temperature, and obtain high-strength corrosion-resistant aluminosilicate glass; the coating liquid thickness is 5μm.
[0063] Comparative Example 2: A method for preparing high-strength, corrosion-resistant aluminosilicate glass: S1: ultrasonically disperse 0.002 g of graphene oxide in deionized water, add 0.1 M sodium hydroxide to adjust the pH to 7.5, add 0.15 g of a chloroform solution of a mercapto quaternary ammonium salt polysiloxane, and ultrasonically disperse for 30-45 min to obtain modified graphene oxide;
[0064] S2: Ultrasonic dispersion of 0.03 g of modified graphene oxide in deionized water to obtain a graphene dispersion with a concentration of 0.003 g / mL; 3.5 mL of tetraethyl orthosilicate was added to 5 mL of ethanol and stirred evenly, 1.5 mL of hydrochloric acid was added, and the mixture was heated to 30°C and stirred for 24 h to obtain a tetraethyl orthosilicate hydrolyzate; 0.05 g of modified graphene oxide, 15 mL of graphene dispersion, and 10 mL of tetraethyl orthosilicate hydrolyzate were placed at 30°C and stirred for 7 h to obtain a coating solution;
[0065] S3: The LAS glass was ultrasonically treated in ethanol, acetone, and deionized water for 15 min in sequence for later use;
[0066] S4: Spin-coat the coating liquid on the surface of LAS glass, heat to 100°C at a heating rate of 2°C / min in a nitrogen atmosphere and keep it warm for 1 hour, continue to heat to 600°C at a heating rate of 2°C / min and keep it warm for 2 hours, cool to room temperature, and obtain high-strength corrosion-resistant aluminosilicate glass; the coating liquid thickness is 5μm.
[0067] Comparative Example 3: A method for preparing high-strength corrosion-resistant aluminosilicate glass: S1: ultrasonically disperse 0.002 g of graphene oxide in deionized water, add 0.1 M sodium hydroxide to adjust the pH to 7.5, add 0.15 g of a chloroform solution of a mercapto quaternary ammonium salt polysiloxane, and ultrasonically disperse for 30-45 min to obtain modified graphene oxide;
[0068] S2: 1 g of modified graphene oxide was added to a dichloromethane solution of 4098-methacrylic acid POSS and 0.15 wt% 2-hydroxy-2-methylacetophenone, irradiated with ultraviolet light for 40 min, washed with ethanol, and dried at 60 ° C to obtain POSS modified graphene oxide; 0.15 g of POSS modified graphene oxide and azobisisobutyronitrile were added to HFO, heated to 85 ° C under a nitrogen atmosphere, 692-(perfluorooctyl)ethyl methacrylate, azobisisobutyronitrile, and HFO mixture were added, and the reaction was kept warm for 1 h, washed with ethanol, and dried at 60 ° C to obtain fluorinated POSS modified graphene oxide;
[0069] S3: Ultrasonic dispersion of 0.03 g of fluorinated POSS modified graphene oxide in deionized water to obtain a graphene dispersion with a concentration of 0.003 g / mL; 3.5 mL of tetraethyl orthosilicate was added to 5 mL of ethanol and stirred evenly, 1.5 mL of hydrochloric acid was added, and the mixture was heated to 30°C and stirred for 24 h to obtain a tetraethyl orthosilicate hydrolyzate; 0.05 g of fluorinated POSS modified graphene oxide, 15 mL of graphene dispersion, and 10 mL of tetraethyl orthosilicate hydrolyzate were placed at 30°C and stirred for 7 h to obtain a coating solution;
[0070] S4: The LAS glass was ultrasonically treated in ethanol, acetone, and deionized water for 15 min in sequence for later use;
[0071] S5: Spin-coat the coating liquid on the surface of LAS glass, heat to 100°C at a heating rate of 2°C / min in a nitrogen atmosphere and keep it warm for 1 hour, continue to heat to 800°C at a heating rate of 2°C / min and keep it warm for 2 hours, cool to room temperature, and obtain high-strength corrosion-resistant aluminosilicate glass; the coating liquid thickness is 5μm.
[0072] Comparative Example 4: A method for preparing high-strength, corrosion-resistant aluminosilicate glass: S1: Ultrasonic dispersion of 0.03 g of graphene oxide in deionized water to obtain a graphene dispersion with a concentration of 0.003 g / mL; 3.5 mL of tetraethyl orthosilicate was added to 5 mL of ethanol and stirred evenly, 1.5 mL of hydrochloric acid was added, and the mixture was heated to 30° C. and stirred for 24 h to obtain a tetraethyl orthosilicate hydrolyzate; 0.05 g of graphene oxide, 15 mL of graphene dispersion, and 10 mL of tetraethyl orthosilicate hydrolyzate were placed at 30° C. and stirred for 7 h to obtain a coating solution;
[0073] S2: The LAS glass was ultrasonically treated in ethanol, acetone, and deionized water for 15 min in sequence and set aside;
[0074] S3: Spin-coat the coating liquid on the surface of LAS glass, heat it to 100°C at a heating rate of 2°C / min in a nitrogen atmosphere and keep it warm for 1 hour, then continue to heat it to 600°C at a heating rate of 2°C / min and keep it warm for 2 hours, and cool it to room temperature to obtain high-strength corrosion-resistant aluminosilicate glass; the coating liquid thickness is 5μm.
[0075] Experiment: Corrosion resistance: Place high-strength corrosion-resistant aluminosilicate glass in a sodium hydroxide alkaline environment for 30 days, take part of the solution and use ICP-OES to analyze the Li + , A1 3+ , Si 4+ Ion concentration is used to evaluate the corrosion resistance of high-strength corrosion-resistant aluminosilicate glass; the experimental data are shown in Table 1 below.
[0076] Table 1 Corrosion resistance test data of high strength corrosion resistant aluminum silicon glass
[0077] <![CDATA[Li + / (mg / L)]]> <![CDATA[Al 3+ / (mg / L)]]> <![CDATA[Si 4+ / (mg / L)]]> Example 1 0.1048 7.1254 6.6445 Example 2 0.0996 6.8974 6.1438 Example 3 0.0954 6.8011 5.8876 Example 4 0.0897 6.6544 5.2547 Comparative Example 1 0.1158 7.6547 7.1898 Comparative Example 2 0.1447 8.9387 7.4487 Comparative Example 3 0.2148 12.4738 10.9644 Comparative Example 4 0.1968 10.2578 9.4587
[0078] Conclusion: The high-strength corrosion-resistant aluminosilicate glass prepared by the present invention has excellent corrosion resistance.
[0079] In Comparative Example 1, the proportion of ethyl orthosilicate in the ethyl orthosilicate hydrolyzate is reduced, resulting in reduced density of the coating layer, the appearance of fine cracks, and reduced corrosion resistance.
[0080] In Comparative Example 2, the modified graphene oxide does not introduce the POSS structure and the fluorinated layer, lacks a rough structure of micropores / mesopores, the interlayer spacing of the graphene oxide is reduced, and there is no fluorinated layer to isolate the alkaline solution, resulting in reduced corrosion resistance.
[0081] In Comparative Example 3, the temperature during the high-temperature curing process was too high, resulting in the breakage of the Si-O-Si bonds formed during the curing process, the cracking of the coating layer, and the reduction of corrosion resistance.
[0082] In Comparative Example 4, unmodified common commercially available graphene oxide was used, and the corrosion resistance was reduced.
[0083] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing high-strength corrosion-resistant aluminosilicate glass, characterized in that: The following steps are involved: S1: Ultrasonic dispersion of fluorinated POSS modified graphene oxide in deionized water to obtain graphene dispersion; adding tetraethyl orthosilicate into ethanol and stirring evenly, adding hydrochloric acid, heating to 30-31°C and stirring for 24h to obtain tetraethyl orthosilicate hydrolyzate; placing fluorinated POSS modified graphene oxide, graphene dispersion and tetraethyl orthosilicate hydrolyzate at 30-31°C and stirring for 7-8h to obtain coating solution; S2: ultrasonically treat the LAS glass in ethanol, acetone, and deionized water for 15-30 min in sequence and set aside; S3: Spin-coat the coating liquid on the surface of LAS glass, heat to 100-101°C in a nitrogen atmosphere and keep it warm for 1-1.5h, continue to heat to 550-650°C and keep it warm for 2-2.5h, and cool to room temperature to obtain high-strength corrosion-resistant aluminosilicate glass.
2. The method for preparing high-strength corrosion-resistant aluminosilicate glass according to claim 1, characterized in that: The preparation method of the fluorinated POSS modified graphene oxide comprises the following steps: Ultrasonic dispersion of graphene oxide in deionized water, adding 0.1 M sodium hydroxide to adjust the pH to 7.5-8, adding a chloroform solution of mercapto quaternary ammonium salt polysiloxane, and ultrasonic dispersion for 30-45 minutes to obtain modified graphene oxide; The modified graphene oxide is added to a dichloromethane solution of 8-methacrylic acid POSS and 0.15-0.2wt% 2-hydroxy-2-methylacetophenone, irradiated with an ultraviolet lamp for 40-45 minutes, washed with ethanol, and dried at 60-65°C to obtain POSS-modified graphene oxide; the POSS-modified graphene oxide and azobisisobutyronitrile are added to HFO, heated to 85-87°C under a nitrogen atmosphere, 2-(perfluorooctyl)ethyl methacrylate, azobisisobutyronitrile and HFO are added, the reaction is kept warm for 1-2 hours, washed with ethanol, and dried at 60-65°C to obtain fluorinated POSS-modified graphene oxide.
3. The method for preparing high-strength corrosion-resistant aluminosilicate glass according to claim 2, characterized in that: In the modified graphene oxide, the mass ratio of graphene oxide to mercapto quaternary ammonium salt polysiloxane is 0.002:(0.15-0.3).
4. The method for preparing high-strength corrosion-resistant aluminosilicate glass according to claim 2, characterized in that: In the POSS modified graphene oxide, the mass ratio of modified graphene oxide: 8-methylallyl POSS is 1: (40-50); in the fluorinated POSS modified graphene oxide, the mass ratio of POSS modified graphene oxide: 2-(perfluorooctyl)ethyl methacrylate is (0.15-0.2): (6-8).
5. The method for preparing high-strength corrosion-resistant aluminosilicate glass according to claim 2, characterized in that: The preparation method of the mercapto quaternary ammonium salt polysiloxane comprises the following steps: Step (1): octamethylcyclotetrasiloxane, γ-chloropropylmethyldiethoxysilane and γ-mercaptopropyltriethoxysilane are added to a reaction vessel and stirred evenly, concentrated sulfuric acid is added, the mixture is heated to 60-65° C. and reacted for 6-8 hours, extracted, the aqueous phase is removed, and rotary evaporation is performed to obtain mercaptochloropropyl polysiloxane; Step (2): adding sodium iodide to acetone and stirring evenly, adding mercaptochloropropyl polysiloxane, heating to 70-75° C. and reflux reaction for 48-50 hours, filtering, rotary evaporation, ether extraction, rotary evaporation, to obtain mercaptoiodopropyl polysiloxane; Step (3): Add mercapto iodopropyl polysiloxane to tetrahydrofuran, add triethylamine, heat to 40-45° C., stir and react for 72-74 hours, rotary evaporate, wash, and dry at 60-65° C. to obtain mercapto quaternary ammonium salt polysiloxane.
6. The method for preparing high-strength corrosion-resistant aluminosilicate glass according to claim 5, characterized in that: In the mercaptochloropropyl polysiloxane, the molar ratio of octamethylcyclotetrasiloxane:γ-chloropropylmethyldiethoxysilane:γ-mercaptopropyltriethoxysilane:concentrated sulfuric acid is 3.5:(2_4):(1-3):3.
5.
7. The method for preparing high-strength corrosion-resistant aluminosilicate glass according to claim 5, characterized in that: In the mercapto iodopropyl polysiloxane, the mass ratio of mercapto chloropropyl polysiloxane to sodium iodide is 4:(0.8-1).
8. The method for preparing high-strength corrosion-resistant aluminosilicate glass according to claim 5, characterized in that: In the mercapto quaternary ammonium salt polysiloxane, the mass ratio of mercapto iodopropyl polysiloxane to triethylamine is 9:(4-5).
9. The method for preparing high-strength corrosion-resistant aluminosilicate glass according to claim 1, characterized in that: The concentration of the graphene dispersion is 0.003-0.005 g / mL; in the tetraethyl orthosilicate hydrolyzate, the volume ratio of tetraethyl orthosilicate: ethanol: hydrochloric acid is (3.5-3.75):5:(1.25-1.5).
10. High-strength corrosion-resistant aluminosilicate glass prepared according to the method for preparing high-strength corrosion-resistant aluminosilicate glass according to any one of claims 1 to 9.
Citation Information
Patent Citations
Textile process and product
CN106061731A
Glass cover plate coating material with ultralow antifriction coefficient, and preparation method thereof
CN110104963A
Preparation method of graphene modified polymer composite material
CN112852076A
Hydrophobic graphene conductive material and preparation method of composite film of hydrophobic graphene conductive material
CN114348995A
Mud-resistant and corrosion-resistant cable material for ships
CN115418046A
Cited By
Wear-resistant and corrosion-resistant metal part and surface treatment process thereof
CN119549378A
Temperature change resistant glass material and preparation method thereof
CN119707308A