Recycled aggregate strengthening method based on carbonized product crystal form control and application
By regulating the crystal form and morphology of the carbonization product, the problem of high water absorption and crushing value of recycled aggregates is solved, and the performance is significantly improved. It is suitable for high-strength concrete and pavement bases under extremely heavy traffic loads.
Patent Information
- Application Number
- CN202410664370.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-27
- Publication Date
- 2024-10-25
AI Technical Summary
Existing recycled aggregate strengthening methods cannot effectively reduce water absorption and crushing value, which limits its large-scale application. In particular, the carbonization modification method is not effective for recycled aggregates with larger diameters.
By adding a crystal form regulator and controlling the carbon dioxide concentration, pressure, temperature and time during the carbonization modification process, the crystal form and morphology of calcium carbonate are controlled to form various forms of calcite and fibrous calcium carbonate, which are filled with recycled aggregates pores and micro-cracks to improve its structural compactness and bonding ability.
Significantly reduces the water absorption and crushing value of recycled aggregates, with a maximum reduction of 88.4% and 61.5%, reaching or approaching the performance standards of natural aggregates, expanding its application fields, including high-strength concrete and pavements under extremely heavy traffic loads Grassroots.
Smart Images

Figure CN118834033A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of strengthening treatment of recycled concrete aggregate, and specifically relates to a recycled aggregate strengthening method based on carbonization product crystal form control and application. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Waste concrete is one of the most difficult solid wastes to utilize. As it is difficult to handle, it is often dumped in the open air, which occupies a large amount of land resources and causes damage to the surrounding environment. Waste concrete contains a large amount of sand and gravel aggregates. Aggregates formed by crushing, screening, grading, cleaning and mixing waste concrete in a certain proportion are called recycled aggregates. Preparing waste concrete into recycled aggregates and adding them to building materials for reuse in the construction field is one of the ways to recycle waste concrete. However, since the surface of recycled aggregates is often covered with a considerable amount of old cement mortar and a large number of microcracks are generated during the crushing process, recycled aggregates have the disadvantages of high water absorption and high crushing value compared with natural aggregates. Water absorption refers to the ratio of the amount of water absorbed by aggregates in a certain period of time to their dry weight. High water absorption leads to high water content, poor fluidity, and reduced strength and durability of concrete. Crushing value refers to the ratio of the weight of the crushed debris measured by the prescribed test method to the total weight of the sample. A large crushing value indicates low aggregate strength. The disadvantages of high water absorption and high crushing value limit the large-scale application of recycled aggregates.
[0004] In order to improve the utilization rate of waste concrete, it is necessary to strengthen the recycled aggregate prepared from waste concrete. At present, the main methods for strengthening recycled aggregates include mechanical grinding, acid treatment, heating grinding, carbonization modification, nanomaterial modification, microbial modification, etc. Among them, carbonization modification is a green and environmentally friendly method for strengthening recycled aggregates. The Chinese patent with the authorization announcement number of CN112125541B (a method for wet carbonization activation of waste concrete recycled micropowder and the application of recycled micropowder) can only strengthen the recycled micropowder with a diameter less than 0.16mm, and cannot strengthen the recycled aggregate with a larger diameter; the Chinese patent with the authorization announcement number of CN112125550B (a method for open carbonization strengthening of waste concrete recycled aggregate) can only reduce the water absorption rate of recycled aggregate by 12.9%, and the improvement of performance is limited. At present, the water absorption rate of other recycled aggregate strengthening methods using carbonization modification can only be reduced by about 20%, and the crushing value can only be reduced by about 10%. The strengthening effect is insufficient, and the water absorption rate and crushing value indicators are still too large, resulting in the inability of recycled aggregates to be applied on a large scale. Summary of the invention
[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a recycled aggregate strengthening method and application based on the crystal form control of carbonization products. By adding a crystal form regulator and controlling the carbon dioxide concentration / pressure, carbonization temperature, carbonization time, stirring speed and other conditions during the carbonization modification process, the directional regulation of the crystal form and morphology of calcium carbonate is achieved, the performance of the recycled aggregate is significantly improved, and the high-quality recycling of waste concrete is promoted.
[0006] In order to achieve the above object, the technical solution of the present invention is:
[0007] In a first aspect, a recycled aggregate strengthening method based on carbonization product crystal form control comprises the following steps:
[0008] S1, pre-processing the waste concrete blocks by crushing and screening, washing and air-drying;
[0009] S2, soaking the recycled aggregate obtained in S1 in a crystal form regulator for 1 to 24 hours;
[0010] S3, contacting the soaked recycled aggregate with tail gas containing 20-100% carbon dioxide concentration, and performing carbonization modification under a carbonization pressure of 100-500 kPa to obtain recycled aggregate based on the crystal form control of the carbonization product;
[0011] Wherein, the crystal form regulator includes: a mixture of Ba(OH)2, ZnCl2, AgNO3 and / or Mg(NO3)2 and water.
[0012] In the second aspect, the recycled aggregate is prepared by the above-mentioned recycled aggregate strengthening method based on the control of the crystal form of the carbonization product.
[0013] In a third aspect, the above-mentioned recycled aggregate strengthening method based on the crystal form control of carbonization products and / or the application of the prepared recycled aggregate include: application in high-strength concrete, or application in pavement base under extremely heavy traffic loads.
[0014] The beneficial effects of the present invention are:
[0015] 1. The present invention adds a crystal modifier to promote the generation of various forms of calcite containing magnesium, barium, iron and / or zinc in the carbonization reaction of the recycled aggregate, which fills the pores and microcracks of the recycled aggregate in a stacking and interweaving manner. At the same time, the rough and uneven surface formed by the stacking and interweaving provides more nucleation sites for the hydration products, promotes the formed hydration products (calcium carbonate, amorphous silica gel, aluminum gel and gypsum, etc.) to fill in the pores and microcracks, makes the recycled aggregate structure dense, effectively reduces the water absorption rate and crushing value, and obtains a recycled aggregate with stronger performance.
[0016] 2. The present invention can directionally control vaterite calcium carbonate and amorphous calcium carbonate with poor thermodynamic stability into fibrous aragonite calcium carbonate, and use the fiber connection ability to improve the interface bonding ability of the recycled aggregate, so as to further improve the quality of the recycled aggregate. It also produces BaCO3, MgCO3 and other precipitates, which together with CaCO3 fill the pores and microcracks of the recycled aggregate, further improving the aggregate strengthening effect.
[0017] 3. Compared with the traditional carbonization method, the performance of the regenerated aggregate is significantly improved by the method of controlling the crystal form of the carbonized product. The water absorption rate can be reduced by 88.4% at most, and the crushing value can be reduced by 61.5% at most. All of them can meet the standards of Class II aggregates, and some can meet the standards of Class I aggregates. The value of the aggregate is significantly improved, and the application field is broad. It can be widely used in the preparation process of high-strength concrete, or in engineering applications such as the construction of road base under extremely heavy traffic loads. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0019] Figure 1 It is a microstructure characterization diagram of comparative example 1 in a specific implementation manner of the present invention.
[0020] Figure 2 It is a microstructure characterization diagram of Example 2 in a specific implementation manner of the present invention. DETAILED DESCRIPTION
[0021] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0022] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0023] A recycled aggregate strengthening method based on carbonization product crystal form control comprises the following steps:
[0024] S1, pre-processing the waste concrete blocks by crushing and screening, washing and air-drying;
[0025] S2, soaking the recycled aggregate obtained in S1 in a crystal form regulator for 1 to 24 hours;
[0026] S3, contacting the soaked recycled aggregate with tail gas containing 20-100% carbon dioxide concentration, and performing carbonization modification under a carbonization pressure of 100-500 kPa to obtain recycled aggregate based on the crystal form control of the carbonization product;
[0027] Wherein, the crystal form regulator includes: a mixture of Ba(OH)2, ZnCl2, AgNO3 and / or Mg(NO3)2 and water.
[0028] The surface of traditional recycled aggregate is originally coated with old cement mortar, and the carbonized products produced after carbonization strengthening are mainly calcium carbonate, amorphous silica gel, aluminum glue and gypsum. Among them, the carbonized product calcium carbonate has multiple forms such as calcite, aragonite, vaterite and amorphous, which have different physical morphologies, grain sizes and solubility. For example, the metastable vaterite type and amorphous calcium carbonate have poor filling effects, which are not conducive to the strengthening of recycled aggregate. The present invention promotes the production of various forms of magnesium, barium, iron or zinc calcite after aggregate carbonization through the addition of crystal form regulators, and fills the pores and microcracks of recycled aggregate by stacking and interweaving, so that the structure of recycled aggregate is dense. At the same time, the rough and uneven surface formed by stacking and interweaving provides nucleation sites for hydration products, promotes the formation of hydration products, fills pores and microcracks, and makes the structure of recycled aggregate more dense. It can also directionally regulate the vaterite calcium carbonate and amorphous calcium carbonate with poor thermodynamic stability into fibrous aragonite calcium carbonate, and use the connecting ability of the fibers to improve the interfacial bonding ability of the recycled aggregate; it also produces precipitates such as BaCO3 and MgCO3, which together with CaCO3 fill the pores and microcracks of the recycled aggregate to further improve the quality of the recycled aggregate.
[0029] Optionally, the ratio of Ba(OH)2, ZnCl2, AgNO3 or Mg(NO3)2 to water is 0.01-0.2 mol / L; the ratio of the added alkali or salt to water can be higher than its solubility. This is because after adding water, a highly fluid liquid can be obtained, which promotes the effective ingredients of the crystal form regulator to fully contact and adhere to the rough surface of the recycled aggregate. At the same time, during wet carbonization, with the continuous reaction of carbon dioxide, the effective ingredients of the crystal form regulator are gradually converted into carbonate precipitates, which promotes the further dissolution of undissolved alkali or salts.
[0030] Optionally, in S1, the crushing and screening pretreatment method is: screening and removing impurities from the waste concrete, and crushing and screening the waste concrete to obtain recycled aggregate with a set particle size.
[0031] Optionally, the crushing methods include: jaw crusher and impact crusher processing crushing.
[0032] Optionally, in S3, the carbonization modification method is wet carbonization, comprising the steps of:
[0033] Industrial tail gas containing 20-100% volume concentration of carbon dioxide is continuously introduced into a crystal form regulator soaked with recycled aggregate to cause carbonization reaction between carbon dioxide and recycled aggregate; the crystal form of carbonized product is controlled by controlling carbon dioxide concentration, carbonization pressure, crystal form regulator temperature, stirring speed and carbonization time; after the carbonization reaction is completed, drying is performed at 60°C to obtain recycled aggregate that has completed carbonization modification.
[0034] Optionally, during wet carbonization, the temperature of the crystal form regulator is controlled at 0-60°C; the stirring rate is 200-800 r / min; the carbonization duration is 0.5-4h, and the stirring container is a reactor.
[0035] Optionally, the industrial tail gas contains carbon dioxide, and may also contain oxygen, nitrogen and / or water vapor, but does not contain other gas components that can react with the crystal form regulator.
[0036] Carbonization pressure refers to the gas pressure above the liquid level of the crystal form regulator.
[0037] Carbonization time refers to the reaction time between recycled aggregate and carbon dioxide immersed in a crystal form regulator at a set temperature while maintaining carbonization pressure.
[0038] In the recycled aggregate prepared by the above-mentioned recycled aggregate strengthening method based on the crystal form control of the carbonized product, due to the suppression of the metastable vaterite type and amorphous calcium carbonate, more calcite containing magnesium, barium, iron and zinc is generated, and these calcites are filled in the pores and microcracks of the recycled aggregate by stacking and interweaving. On the other hand, the fibrous aragonite calcium carbonate originally dispersed between the vaterite type and the amorphous calcium carbonate is transformed into a state of bridging between the calcites, so that the interface bonding ability of the raw aggregate is further improved.
[0039] The above-mentioned recycled aggregate strengthening method based on the crystal form control of the carbonized product and / or the application of the prepared recycled aggregate include: application in high-strength concrete or pavement base under extremely heavy traffic loads.
[0040] In the following examples, the crushing values and water absorption of natural aggregate and recycled aggregate were tested according to the relevant test methods in "Recycled Coarse Aggregate for Concrete" GB / T 25177-2010. The main physical properties of the untreated recycled aggregate are: water absorption 8.25%, crushing value 23.0%; the main physical properties of the selected natural aggregate are: water absorption 0.88%, crushing value 8.66%. It can be seen that the main physical properties of recycled aggregate are quite different from those of natural aggregate.
[0041] Example 1
[0042] A recycled aggregate prepared by a recycled aggregate strengthening method based on the crystal form control of carbonized products, the preparation method comprising the following steps:
[0043] (1) The waste concrete from the construction waste disposal site is screened and impurities are removed, and then crushed by a jaw crusher and an impact crusher. Finally, the recycled aggregate with a particle size of less than 31.5 mm is obtained by screening, and then rinsed and naturally air-dried to constant weight.
[0044] (2) The recycled aggregate that has been air-dried to a constant weight is placed in a crystal modifier and soaked for 4 hours. The crystal modifier contains Ba(OH)2, and the mixing ratio of Ba(OH)2 to water is 0.1 mol / L.
[0045] (3) After the set soaking time, industrial tail gas with a carbon dioxide concentration of 80% is introduced into the liquid soaked with recycled aggregate, the carbonization pressure is 300 kPa, the liquid temperature is controlled at 20°C, the stirring speed is 400 r / min, and the stirring is continued for 2 hours.
[0046] (4) Rinse the carbonized recycled aggregate and allow it to air dry to constant weight.
[0047] Example 2
[0048] The difference from Example 1 is that in step (2), in the crystal form regulator, the mixing ratio of the active ingredient and water is: 0.1 mol / L Ba(OH)2 and 0.1 mol / L Mg(NO3)2.
[0049] Example 3
[0050] The difference from Example 1 is that in step (2), in the crystal form regulator, the mixing ratio of the active ingredient and water is: 0.1 mol / L Ba(OH)2, 0.1 mol / L Mg(NO3)2, 0.1 mol / L ZnCl2 and 0.1 mol / L AgNO3, containing a total of 0.4 mol / L of metal elements.
[0051] Example 4
[0052] The difference from Example 2 is that in step (3), industrial tail gas with a carbon dioxide concentration of 60% is introduced into the liquid soaked with the recycled aggregate.
[0053] Example 5
[0054] The difference from Example 2 is that in step (3), industrial tail gas with a carbon dioxide concentration of 99% is introduced into the liquid soaked with the recycled aggregate.
[0055] Example 6
[0056] The difference from Example 2 is that in step (3), the carbonization pressure is 100 kPa.
[0057] Example 7
[0058] The difference from Example 2 is that in step (3), the carbonization pressure is 500 kPa.
[0059] Example 8
[0060] The difference from Example 2 is that in step (3), the liquid temperature is controlled at 0°C.
[0061] Example 9
[0062] The difference from Example 2 is that in step (3), the liquid temperature is controlled at 40°C.
[0063] Example 10
[0064] The difference from Example 2 is that in step (3), the stirring speed is 200 r / min.
[0065] Embodiment 11
[0066] The difference from Example 2 is that in step (3), the stirring speed is 800 r / min.
[0067] Example 12
[0068] The difference from Example 2 is that in step (3), the duration is 0.5 h.
[0069] Embodiment 13
[0070] The difference from Example 2 is that in step (3), the process lasts for 4 hours.
[0071] Comparative Example 1
[0072] The difference from Example 1 is that in step (2), the recycled aggregate air-dried to constant weight is soaked in pure water for 4 hours.
[0073] The recycled aggregates produced in Example 2 and Comparative Example 1 were characterized, and the electron microscopy results are as follows: Figure 1 and Figure 2 As shown, Figure 1 The electron microscope image of Comparative Example 1 is shown. Figure 2 The electron microscope image of Example 2 is shown.
[0074] Different positions of the recycled aggregates strengthened by carbonization were immersed in pure water. Figure 1 (a) and Figure 1 As shown in (b), it can be seen that the carbonization products are relatively small. Figure 1 The metastable vaterite type and Figure 1(b) is mainly amorphous, and the carbonization product is mainly composed of calcium carbonate, which is loosely distributed and has a poor filling effect. Figure 1 (a) and Figure 1 In the center of image (b), obvious cracks can be seen, which means that there are still large microcracks on the surface of the recycled aggregate.
[0075] The recycled aggregate prepared by the present invention is as follows Figure 2 As shown, Figure 2 (a)~ Figure 2 (d) for different locations; Figure 2 (a) and Figure 2 As shown in (c), various forms of calcite containing magnesium, barium, iron and / or zinc are generated on the recycled aggregate and filled in the recycled aggregate by stacking and interweaving. Figure 2 (a) Microcracks and Figure 2 (c) in the pores; Figure 2 (b) shows that the proportion of metastable vaterite and amorphous calcium carbonate is significantly reduced; Figure 2 (d) It shows that the fibrous aragonite calcium carbonate connects the interface transition zone between the aggregate and the mortar and plays a bridging role, thereby enhancing the bonding properties of the interface transition zone.
[0076] According to the relevant test methods in "Recycled Coarse Aggregate for Concrete" GB / T 25177-2010, the crushing value and water absorption rate of natural aggregate, unreinforced recycled aggregate, and recycled aggregate treated by the above-mentioned reinforcement method were tested. The test results are shown in Table 1.
[0077] Table 1
[0078] type Water absorption / % Water absorption rate change / % Crushing value / % Crushing value change rate / % Natural Aggregates 0.88 - 8.66 - Unreinforced Aggregate 8.25 - 23.0 - Example 1 1.16 85.9 8.92 61.2 Example 2 0.96 88.4 8.85 61.5 Example 3 1.06 87.2 9.96 61.0 Example 4 1.24 85.0 9.23 59.9 Example 5 1.02 87.6 9.07 60.6 Example 6 1.15 86.1 9.16 60.2 Example 6 1.26 84.7 9.28 59.7 Example 8 1.00 87.9 9.01 60.8 Example 9 1.28 84.5 9.32 59.5 Example 10 1.40 83.0 10.23 55.5 Embodiment 11 1.83 77.8 11.58 49.7 Example 12 1.98 76.0 11.87 48.4 Embodiment 13 1.59 80.7 10.46 54.5 Comparative Example 1 5.34 35.3% 18.12 21.2%
[0079] The calculation method of the water absorption rate change rate is: water absorption rate change rate = (water absorption rate of unreinforced aggregate - water absorption rate of embodiment) / water absorption rate of unreinforced aggregate;
[0080] The calculation method of the crushing value change rate is: crushing value change rate = (unreinforced aggregate crushing value - embodiment crushing value) / unreinforced aggregate crushing value.
[0081] As can be seen from Table 1, the water absorption and crushing value of the recycled aggregates are significantly reduced based on the carbonization product crystal form control method. Compared with the unreinforced aggregates, the water absorption is reduced by 88.4% (the water absorption of Example 2 is 0.96%), and the crushing value is reduced by 61.5% (the crushing value of Example 2 is 8.85%), reaching the Class I aggregate standard. Under other strengthening methods, the aggregates all reach the Class II aggregate standard. The quality of recycled aggregates is significantly improved, and they can completely replace natural aggregates in high-strength concrete and road bases under extremely heavy traffic loads, thereby realizing the large-scale application of waste concrete.
[0082] Embodiment 14
[0083] The reinforced recycled aggregate in the above Example 2 was used as raw material, and no natural aggregate was used to prepare C60 grade high-strength concrete, which was poured and cured to obtain the test piece of Example 14.
[0084] Comparative Example 2
[0085] Using natural aggregates of the same grade and proportion as the recycled aggregates in Example 14, a C60 grade high-strength concrete was prepared by the same method as in Example 14 to obtain Comparative Example 2.
[0086] The mechanical properties of Example 14 and Comparative Example 2 were measured, and the results are shown in Table 2.
[0087] Table 2
[0088]
[0089] It can be seen from Table 2 that the strength indicators of C60 grade high-strength concrete prepared by using the strengthened recycled aggregate and natural aggregate are not much different, and the indicators of Example 14 meet the standard requirements. Therefore, the recycled aggregate strengthening method based on the crystal form control of the carbonization product proposed in the present invention is adopted to significantly improve the quality of the recycled aggregate, which can be used to prepare high-strength concrete, specifically, to prepare high-strength concrete of C60 and above.
[0090] Embodiment 15
[0091] The recycled aggregate reinforced by Example 2 was prepared according to the Technical Specifications for Highway Pavement Base Construction.
[0092] (JTG / T F20-2015) specification requirements, prepare an inorganic binder stabilized base, the cement content is 5%, the aggregate grading is 20-30mm:10-20mm:5-10mm:0-5mm=18:35:15:32, the compaction degree is 98%, and the static pressure method is used to form an unconfined compressive strength specimen with a diameter of 150mm to obtain Example 15.
[0093] Comparative Example 3
[0094] Using natural aggregates of the same grade as in Example 15 as raw materials, an unconfined compressive strength specimen with a diameter of 150 mm was prepared by the same method as in Example 15 to obtain Comparative Example 3.
[0095] The properties of Example 15 and Comparative Example 3 were measured, and the results are shown in Table 3.
[0096] Table 3
[0097]
[0098] It can be seen from Table 3 that by adopting the recycled aggregate strengthening method based on the crystal form control of carbonization products proposed in the present invention, the 7d unconfined compressive strength of the cement-stabilized all-recycled aggregate pavement base can reach 6.5MPa, which meets the strength requirement of 5.0-7.0MPa under extremely heavy and extra-heavy traffic on expressways and first-class highways; the recycled aggregate of the present invention can replace natural crushed stone and be applied to the construction of transportation infrastructure, especially in the pavement base under extremely heavy traffic loads, which can improve the utilization rate of waste concrete and greatly reduce the project cost, and has important social and economic benefits.
[0099] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A recycled aggregate strengthening method based on the crystal form control of carbonization products, It is characterized in that The following steps are involved: S1, pre-processing the waste concrete blocks by crushing and screening, washing and air-drying; S2, soaking the recycled aggregate obtained in S1 in a crystal form regulator for 1 to 24 hours; S3, contacting the soaked recycled aggregate with tail gas containing 20-100% carbon dioxide concentration, and performing carbonization modification under a carbonization pressure of 100-500 kPa to obtain recycled aggregate based on the crystal form control of the carbonization product; Wherein, the crystal form regulator includes: Ba(OH) 2 、ZnCl 2 AgNO 3 and / or Mg(NO 3 ) 2 Mixture with water.
2. The recycled aggregate strengthening method based on the carbonization product crystal form control according to claim 1, It is characterized in that The Ba(OH) 2 、ZnCl 2 AgNO 3 or Mg(NO 3 ) 2 The ratio with water is 0.01~0.2mol / L.
3. The recycled aggregate strengthening method based on the carbonization product crystal form control according to claim 1, It is characterized in that In S1, the crushing and screening pretreatment method is: the waste concrete is screened and impurities are removed, and then crushed and screened to obtain recycled aggregate with a set particle size.
4. The recycled aggregate strengthening method based on the carbonization product crystal form control according to claim 3, It is characterized in that Crushing methods include: jaw crusher and impact crusher.
5. The recycled aggregate strengthening method based on the carbonization product crystal form control according to claim 1, It is characterized in that In S3, the carbonization modification method is wet carbonization.
6. The recycled aggregate strengthening method based on the carbonization product crystal form control according to claim 4, It is characterized in that The wet carbonization method is: Industrial tail gas containing 20-100% volume concentration of carbon dioxide is continuously introduced into a crystal form regulator soaked with recycled aggregate to cause carbonization reaction between carbon dioxide and recycled aggregate; the crystal form of carbonized product is controlled by controlling carbon dioxide concentration, carbonization pressure, crystal form regulator temperature, stirring speed and carbonization time; after the carbonization reaction is completed, drying is performed at 60°C to obtain recycled aggregate that has completed carbonization modification.
7. The recycled aggregate strengthening method based on the carbonization product crystal form control according to claim 5, It is characterized in that The temperature of the crystal form regulator is controlled at 0-60°C; the stirring rate is 200-800r / min; the carbonization duration is 0.5-4h, and the stirring container is a reactor.
8. The recycled aggregate strengthening method based on the carbonization product crystal form control according to claim 5, It is characterized in that Industrial off-gases contain carbon dioxide, oxygen, nitrogen and / or water vapour.
9. A recycled aggregate prepared by the recycled aggregate strengthening method based on the carbonization product crystal form control as claimed in any one of claims 1 to 8.
10. A recycled aggregate strengthening method based on carbonization product crystal form control as claimed in any one of claims 1 to 8 and / or a use of the recycled aggregate as claimed in claim 9, It is characterized in that The applications include: application in high-strength concrete; or application in road base under extremely heavy traffic loads.
Citation Information
Patent Citations
Method for carbon dioxide strengthening of recycled concrete aggregate
CN104045251A
Preparation method of carbonized concrete capable of regulating and controlling crystal form of carbonized product and low-carbon concrete
CN115340332A
Method for capturing CO2 by calcium silicate and synchronously condensing into high-breaking-strength material
CN115536321A
Heating-carbonization strengthening method for improving carbonization depth of recycled aggregate
CN117682783A
Method of modifying regenerated aggregate
JP2005001895A
Cited By
Reinforced ardealite aggregate, ultra-high performance concrete material and preparation method of ultra-high performance concrete material
CN119898978A
Conductive fiber reinforced concrete and preparation method thereof
CN120365013A
Method for controllably preparing nanoscale calcium carbonate by taking regenerated micro powder as calcium source
CN122212213A