A wear-resistant ball valve ball spraying device and supersonic spraying process

By designing wear-resistant ball valve ball spraying device and supersonic spraying process, the problem of poor binding performance of ball coating of large-diameter ball valve ball is solved, and a coating with high hardness and high binding force is achieved, meeting the needs of wear resistance and sealing , improves production efficiency and product quality.

CN118835191BActive Publication Date: 2024-12-03SICHUAN SUKE FLUID CONTROL EQUIP CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411330901.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-03
Estimated Expiration
2044-09-24

AI Technical Summary

Technical Problem

During the spraying process, the large-diameter ball valve ball has poor coating bonding performance due to uneven flame temperature, which is prone to cracking or falling off, and cannot meet the wear resistance and sealing requirements under high-speed fluid erosion and solid particles impact.

Method used

A wear-resistant ball valve ball spraying device is designed, including a base, spindle box, feeding mechanism, spraying assembly and processing technology components. It adopts supersonic spraying process and preheating and cooling treatment steps, and uses Cr3C2-25NiCr-SiC mixing. Powder, adjust the distance between the flame nozzle and the sphere and spray parameters to ensure the uniformity and hardness of the coating.

Benefits of technology

The coating is achieved with high hardness (900HV~1050HV), low porosity (≤1%) and high binding force (≥80MPa), which enhances impact and wear resistance and ensures the sealing performance and production efficiency of the sphere.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118835191B_ABST
    Figure CN118835191B_ABST
Patent Text Reader

Abstract

The present invention discloses a wear-resistant ball valve sphere spraying device and a supersonic spraying process, which belong to the field of metal surface spraying technology, and aim to solve the technical problem of coating cracking or falling off caused by poor bonding performance between the surface coating of a large-caliber ball valve sphere and the workpiece surface in the prior art. It includes a base, a spindle box and a feeding mechanism respectively arranged on the base; the spindle box is provided with a spindle for driving the ball valve sphere to be processed to rotate; the feeding mechanism includes a guide rail arranged on the base and a feeding rack movably connected to the guide rail; the feeding rack is provided with a feeding rod coaxially arranged with the spindle and used for inserting and fixing the sphere; the base is respectively provided with a spraying assembly and a processing assembly; the spraying assembly and the processing assembly both act on the sphere. The wear-resistant ball valve sphere spraying device and the supersonic spraying process provided by the present invention can effectively improve the production efficiency of the ball valve sphere, improve the stability of product quality, and reduce production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal surface spraying, and in particular to a wear-resistant ball valve ball spraying device and a supersonic spraying process. Background Art

[0002] Wear-resistant ball valves are widely used in many key industries such as polysilicon, organic silicon, petrochemicals, coal chemical industry, etc. due to their excellent wear resistance, sealing, erosion resistance and corrosion resistance. Wear-resistant ball valves require the use of hard alloys with sufficient hardness for wear-resistant coating and surface treatment to ensure that the valve can maintain good wear resistance, erosion resistance and sealing under high-speed fluid erosion and solid particle impact.

[0003] During the spraying process of large-diameter spheres, the flame temperature has local accumulation, the thickness of the sphere is thick and uneven, and the flame cannot heat the surface and interior of the sphere evenly during the spraying process. During the spraying process, the natural cooling can easily cause uneven heating of the sphere surface, resulting in a decrease in local bonding strength, and the final cemented carbide coating is prone to cracking or falling off.

[0004] Therefore, there is an urgent need for a spraying device and a surface spraying process for a large-caliber ball valve ball. Summary of the invention

[0005] The purpose of the present invention is to provide a wear-resistant ball valve ball spraying device and a supersonic spraying process to solve the technical problem of coating cracking or falling off caused by poor bonding performance between the surface coating of a large-diameter ball valve ball and the workpiece surface in the prior art.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a wear-resistant ball valve ball spraying device, comprising a base, and a spindle box and a feeding mechanism respectively arranged on the base;

[0008] The spindle box is provided with a spindle for driving the ball of the ball valve to be processed to rotate;

[0009] The feeding mechanism comprises a guide rail arranged on the base and a feeding frame movably connected to the guide rail; the feeding frame is provided with a feeding rod coaxially arranged with the main shaft and used for inserting and fixing the ball;

[0010] The base is provided with a spraying component and a processing component respectively; the spraying component and the processing component both act on the sphere.

[0011] Optionally or preferably, the spraying assembly includes a spraying device and a spraying bracket for fixing the spraying device; the spraying bracket is movably connected to the base;

[0012] The processing technology assembly includes a plurality of flame nozzles, a plurality of cooling tubes and a fixing bracket for fixing the flame nozzles and the cooling tubes; the fixing bracket is movably connected to the base;

[0013] The plurality of flame nozzles and the plurality of cooling pipes are arranged crosswise and at intervals.

[0014] Optionally or preferably, the distance between the spray head of the spraying device and the sphere is L , L 350mm-450mm;

[0015] The spacing between adjacent flame nozzles is M 1, M 1 is 150mm-250mm; the distance between the flame nozzle and the sphere is M 2, M 2 is 150mm-250mm.

[0016] A supersonic spraying process for a wear-resistant ball valve ball comprises the following steps:

[0017] S1, rough machining and surface treatment, and placing samples on the sphere;

[0018] S2, preheating, preheating the surface-treated sphere to improve the bonding performance between the coating material and the sphere surface;

[0019] S3, supersonic spraying, selecting a spraying material, and performing supersonic spraying on the outer circle of the sphere through a spraying device;

[0020] S4, cooling treatment, remove the outer circle of the ball from the wear-resistant ball valve ball spraying device, and place it in an insulation box for slow cooling treatment;

[0021] S5. Keep the sample block, grind the weld point of the sample block and remove the sample block for bonding rate, porosity, hardness testing and keep it for future reference;

[0022] S6, the post-treatment process of the outer coating of the sphere is to spray the outer coating of the sphere to ensure the coating quality.

[0023] Optionally or preferably, the method for rough machining the outer circle of the sphere in S1 is: rough machining the outer circle of the sphere forging blank into a shape with an outer diameter smaller than 0.8 mm of the size of the finished part drawing;

[0024] The method of arranging the sample blocks on the outer circle of the sphere in S1 is: spot welding the sample blocks at the non-matching and sealing positions on the outer circle of the sphere, and the number of the sample blocks is not less than 6;

[0025] The method for surface treatment of the outer circle of the sphere in S1 comprises the following steps:

[0026] S11, cleaning the outer circle of the rough-machined sphere with an environmentally friendly solvent-based cleaning agent to remove surface oil stains;

[0027] S12, performing sandblasting roughening treatment on the outer cylindrical surface of the sphere after rough machining, the sandblasting material is white corundum sand, the particle size is 24 mesh-28 mesh, the sandblasting pressure is 0.6 MPa, the sandblasting distance is 100 mm, and the sandblasting moving speed is 200 mm / s-400 mm / s;

[0028] S13. After sandblasting is completed, use a black light to check to ensure that there is no oil fluorescence in the sprayed area on the outer surface of the sphere.

[0029] Optionally or preferably, the method for preheating the outer circle of the surface-treated sphere in S2 is: placing the outer circle of the sphere in a heating box for preheating, raising the temperature to 110° C. to 130° C., and keeping the temperature for not less than 1h / 25mm;

[0030] The interval between the treatment and preheating of the outer surface of the sphere shall not exceed 12 minutes to prevent contamination of the outer surface of the sphere.

[0031] Optionally or preferably, the method of supersonic spraying the outer circle of the sphere by a spraying device in S3 comprises the following steps:

[0032] S31, select the spraying material as Cr3C2-25NiCr-SiC mixed powder with a particle size of 20μm-55μm;

[0033] S32. Clamp the outer circle of the ball on the wear-resistant ball valve ball spraying device. The interval from preheating to clamping should not exceed 20 minutes.

[0034] S33, adjust the distance between the flame nozzle and the outer circle of the sphere so that the distance between the flame nozzle and the outer circle of the sphere M 2 is 150mm-250mm; adjust the flame nozzle to the oblique lower side opposite to the spray nozzle of the spray device and ignite it. By controlling the size of the flame sprayed by the flame nozzle, the temperature of the outer surface of the sphere is ensured to be uniform;

[0035] S34, selecting a plurality of temperature layer measurement points on the outer surface of the sphere to measure the outer surface temperature of the sphere; when the outer surface temperature of the sphere is between 80°C and 100°C, starting supersonic spraying;

[0036] When the outer surface temperature of the sphere is greater than 150°C, stop spraying and cool it through the cooling pipe; continue spraying when it cools to 80°C-100°C; introduce nitrogen at room temperature into the cooling pipe;

[0037] S35. When the outer diameter of the sphere is larger than 0.8mm of the size of the finished product drawing, spraying is completed.

[0038] Optionally or preferably, the method of selecting multiple temperature interlayer measurement points in S34 is: setting them on one side close to the nozzle of the spraying device, and the number of them set on the same horizontal line is not less than 3, and the number of layers set in the longitudinal direction is not less than 3;

[0039] When supersonic spraying is performed on the outer circle of the sphere in S34, the relative running speed between the nozzle of the spraying device and the outer circle of the sphere is 450mm / s-550mm / s; the distance between the nozzle of the spraying device and the outer circle of the sphere L It is 350mm-450mm; the fuel flow rate is 6.5GPH-7GPH; the oxygen flow rate is 1900SCFH-1950SCFH; the nitrogen flow rate is 25SCFH; and the powder feeding speed is 7r / min.

[0040] Optionally or preferably, the method for cooling the outer circle of the sphere after spraying in S4 is: heat preservation and slow cooling, and the cooling time is 2h / 25mm.

[0041] Optionally or preferably, the post-treatment process of the outer coating of the sphere in S6 comprises the following steps:

[0042] S61, coating inspection;

[0043] S62, grinding, using a spherical grinder to grind the outer circle of the sphere, the grinding size is the size of the fine part drawing, and the surface after grinding is uniform in metallic color, without black skin or other spots;

[0044] S63, coarse grinding, use W40 boron carbide / silicon carbide grinding paste to match the valve seat for coarse grinding, the grinding time is 2h-4h, until no grinding lines can be observed on the coating surface;

[0045] S64, fine grinding, use W14 diamond grinding paste to grind with the matching valve seat manually on a rotating grinding platform, and compare every 10 minutes until the sealing surface roughness reaches 0.8;

[0046] When the sealing surface roughness reaches 0.8, use W3.5 diamond grinding paste for fine grinding, and compare every 10 minutes until the roughness reaches above 0.2;

[0047] S65, polishing, use W0.5 diamond grinding paste to polish manually on a rotating grinding platform, compare every 10 minutes, and the product will be a mirror surface after polishing;

[0048] S66. Leak detection. The method of leak detection is:

[0049] S661. Remove the grinding residue in kerosene and clean the outer circle of the ball and the valve seat;

[0050] S662. Fix the outer circle of the sphere to keep the outer circle flow passages of the sphere parallel; place the valve seat on the outer circle of the sphere to ensure that the surrounding sealing surfaces fit tightly;

[0051] S663, penetration test: Pour kerosene into the valve seat flow channel and observe for 15 minutes. If there is no kerosene leakage, it is qualified; otherwise, repeat step S64 and pour kerosene again for observation;

[0052] S664, air blowing test: compressed air is used to blow the contact area between the outer spherical surface of the ball and the valve seat. It is qualified if there is no bubble;

[0053] S665, flip the outer circle of the ball 180 degrees and fix it again, replace another valve seat and repeat steps S661 to S664;

[0054] S666. When the penetration test and blowing test of the corresponding spherical surfaces of the two valve seats are qualified, the inspection is completed and the grinding is qualified.

[0055] Based on the above technical solution, the present invention can at least produce the following technical effects:

[0056] The wear-resistant ball valve ball spraying device provided by the present invention can, on the one hand, reliably and stably clamp the ball; on the other hand, it can well match the ball supersonic spraying process provided by the present invention, and the relative positions of the flame nozzle, the cooling pipe and the spraying device and the outer circle of the ball are easy to adjust, so as to obtain a better spraying effect;

[0057] The invention provides a supersonic spraying process for a wear-resistant ball valve ball, which adopts Cr3C2-25NiCr-SiC mixed powder and a special hardening parameter process so that the coating hardness can reach 900HV~1050HV (66HRC~70HRC), the porosity is ≤1%, and the bonding force is ≥80MPa, which meets the requirements of most existing wear-resistant working conditions and has market applicability;

[0058] Preheating before spraying can effectively prevent local deformation of the sphere caused by uneven heating during the spraying process and the impact on poor coating adhesion;

[0059] The use of low-temperature spraying control during the spraying process can reduce the degree of oxidation and decarburization of the coating, thereby enhancing the toughness of the coating and having higher impact resistance and wear resistance;

[0060] The heat preservation and slow cooling process after spraying can effectively eliminate the mechanical stress of the ball generated during the spraying process and the local deformation of the ball after grinding and storage, thereby ensuring the sealing performance of the ball and the valve seat;

[0061] In the post-processing process of spray coating, the implementation of grinding, lapping and polishing processes can effectively ensure the one-time qualified rate of products. The setting of constant parameters can effectively improve production efficiency, improve product quality stability, reduce production costs, and form standardized production.

[0062] The dual leakage detection method of penetration test and air blowing test can effectively prevent unqualified products from flowing into the next process and causing assembly rework, which can effectively improve the first-time qualified rate of assembly. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 is a front view structural schematic diagram of the first embodiment of the present invention;

[0064] Figure 2 is a schematic diagram of a top view of the structure of the first embodiment of the present invention;

[0065] Figure 3 This is a schematic diagram of sample block layout in Embodiment 1 of the present invention;

[0066] Figure 4 It is a schematic diagram of the layout of temperature interlayer measurement points in the first embodiment of the present invention;

[0067] Figure 5 It is a flow chart of the second embodiment of the present invention.

[0068] In the figure: 1. base; 2. spindle box; 3. loading rack; 4. spindle; 5. sphere; 6. loading rod; 7. spraying device; 8. flame nozzle; 9. cooling pipe; 10. sample block; 11. temperature interlayer measurement point. DETAILED DESCRIPTION

[0069] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments, and all other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making creative work belong to the scope of protection of the present invention.

[0070] Embodiment 1:

[0071] See also Figures 1 to 4 A wear-resistant ball valve ball spraying device comprises a base 1 and a spindle box 2, a feeding structure, a spraying component and a processing component respectively arranged on the base 1; wherein the spindle box 2 is provided with a spindle 4 for driving the ball valve ball 5 to be processed to rotate.

[0072] In this embodiment, the feeding mechanism comprises a guide rail disposed on the base 1 and a feeding frame 3 movably connected to the guide rail; the feeding frame 3 is provided with a feeding rod 6 coaxially disposed with the main shaft 4 and used for inserting and fixing the sphere.

[0073] In this embodiment, the spraying assembly includes a spraying device 7 and a spraying bracket for fixing the spraying device 7; wherein the spraying device 7 is a supersonic spraying device JP8000.

[0074] The processing technology component includes three flame nozzles 8, four cooling tubes 9 and a fixing bracket for fixing the flame nozzles 8 and the cooling tubes 9; specifically, the spacing M1 between the three flame nozzles 8 is 200 mm; the cooling tubes 9 and the flame nozzles 8 are arranged crosswise and at intervals, and the four cooling tubes 9 are combined in pairs and respectively arranged in the intervals between the three flame nozzles 8. In this embodiment, the content of the cooling tubes 9 is nitrogen at room temperature.

[0075] In order to conveniently adjust the distance between the nozzle of the spray device 7, the flame nozzle 8 and the cooling tube 9 and the outer circle of the sphere 5, the above-mentioned spray bracket and the fixed bracket are slidably connected to the upper end surface of the base 1 (not shown in the figure); it can be understood that the base 1 is also provided with corresponding slide rails and limiting mechanisms for achieving the above-mentioned effects of the spray bracket and the fixed bracket.

[0076] Embodiment 2:

[0077] See also Figure 5 This embodiment provides a supersonic spraying process for a wear-resistant ball valve ball based on the first embodiment, that is, the wear-resistant ball valve ball spraying device provided in the first embodiment is used to perform supersonic spraying on the ball valve ball, including the following steps:

[0078] S1, rough machining and surface treatment, and placing a sample block 10 on the sphere 5;

[0079] The method for arranging the sample blocks 10 on the sphere 5 is as follows: spot welding the sample blocks 10 at the non-matching and sealing positions of the sphere 5, and the number of the sample blocks 10 is 6 (eg Figure 3 shown);

[0080] The above method for surface treatment of the sphere 5 comprises the following steps:

[0081] S11, cleaning the rough-machined sphere 5 with an environmentally friendly solvent-based cleaning agent to remove surface oil stains;

[0082] S12, performing sandblasting roughening treatment on the surface of the rough-machined sphere 5, the sandblasting material is white corundum sand, the particle size is 24 mesh-28 mesh, the sandblasting pressure is 0.6 MPa, the sandblasting distance is 100 mm, and the sandblasting moving speed is 200 mm / s-400 mm / s;

[0083] It should be noted that the non-sprayed area near the sprayed surface needs to be protected and can be blocked with heat-resistant glass cloth or asbestos.

[0084] S2, preheating, preheating the surface-treated sphere 5 to improve the bonding performance between the coating material and the surface of the sphere 5;

[0085] The above-mentioned method for preheating the surface-treated sphere 5 is: placing the sphere 5 in a heating box for preheating, heating it to 120°C, and keeping it warm for not less than 1h / 25mm; the interval between the surface treatment and preheating of the sphere 5 does not exceed 12min to prevent the surface of the sphere 5 from being contaminated.

[0086] Among them, 1h / 25mm means that every 25mm of workpiece thickness requires 1 hour of cooling.

[0087] In this embodiment, preheating before spraying can effectively prevent local deformation of the sphere caused by uneven heating during the spraying process and the influence on poor coating adhesion.

[0088] S3, supersonic spraying, selecting a spraying material, and performing supersonic spraying on the sphere 5 through the spraying device 7;

[0089] In this embodiment, the method of supersonic spraying of the sphere 5 by the spraying device 7 comprises the following steps:

[0090] S31, select the spraying material as Cr3C2-25NiCr-SiC mixed powder with a particle size of 20μm-55μm;

[0091] S32, clamp the ball 5 on the wear-resistant ball valve ball spraying device, and the interval from preheating to clamping completion shall not exceed 20 minutes;

[0092] S33, adjust the distance between the flame nozzle 8 and the outer circle of the sphere 5, so that the distance between the flame nozzle 8 and the sphere 5 M 2 is 200mm; the flame nozzle 8 is adjusted to the lower side opposite to the nozzle of the spraying device 7 and then ignited, and the size of the spraying flame of the flame nozzle 8 is controlled to ensure that the surface temperature of the sphere 5 is uniform;

[0093] S34, selecting a plurality of temperature interlayer measurement points 11 on the surface of the sphere 5 to measure the surface temperature of the sphere 5; when the surface temperature of the sphere 5 is between 80° C. and 100° C., starting supersonic spraying;

[0094] In this embodiment, the parameters of supersonic spraying are set as follows: the relative running speed between the nozzle of the spraying device 7 and the sphere 5 is 500 mm / s; the distance between the nozzle of the spraying device 7 and the sphere 5 is L The fuel flow rate is 6.5GPH-7GPH; the oxygen flow rate is 1900SCFH-1950SCFH; the nitrogen flow rate is 25SCFH; and the powder feeding speed is 7r / min.

[0095] The arrangement method of the temperature interlayer measurement points 11 is as follows: the temperature interlayer measurement points 11 are arranged on the side close to the nozzle of the spraying device 7, and the number of the temperature interlayer measurement points 11 arranged on the same horizontal line is not less than 3, and the number of the temperature interlayer measurement points 11 arranged in the longitudinal direction is not less than 3 (such as Figure 4 as shown).

[0096] When the surface temperature of the sphere 5 is greater than 150°C, stop spraying and cool it through the cooling pipe 9; continue spraying when it cools to 80°C-100°C; introduce nitrogen at room temperature into the cooling pipe 9;

[0097] In this embodiment, the use of low-temperature spraying control during the spraying process can reduce the degree of oxidation and decarburization of the coating, thereby enhancing the toughness of the coating and having higher impact resistance and wear resistance.

[0098] S35. When the outer diameter of the sphere 5 is larger than 0.8 mm of the size on the finished product drawing, spraying is completed.

[0099] S4, cooling treatment, removing the ball 5 from the wear-resistant ball valve ball spraying device and placing it in an insulation box for slow cooling treatment;

[0100] In this embodiment, the cooling treatment method for the sphere 5 after spraying is insulation and slow cooling, and the slow cooling time is 2h / 25mm; the insulation and slow cooling process can effectively eliminate the mechanical stress generated by the sphere during the spraying process, and effectively eliminate the local deformation phenomenon of the sphere during storage after grinding, thereby ensuring the sealing performance of the sphere and the valve seat.

[0101] Among them, 2h / 25mm means that every 25mm of workpiece thickness requires 2 hours of cooling.

[0102] S5, retain the sample block 10, grind the welding point position of the sample block 10 and remove the sample block 10 for bonding rate, porosity, hardness testing and keep it for future reference;

[0103] S6, post-treatment process of the coating of the sphere 5, spraying post-treatment of the coating of the sphere 5 to ensure the coating quality.

[0104] In this embodiment, the coating post-treatment process of the sphere 5 includes the following steps:

[0105] S61, coating inspection, spray hardness can reach 900HV0.3-1050HV0.3 (66HRC-70HRC), porosity ≤1%, bonding strength ≥80MPa;

[0106] S62, grinding, using a spherical grinder to grind the outer circle of the sphere 5, the grinding size is the size of the fine part drawing, and the surface after grinding is uniform in metallic color without black skin or other spots;

[0107] S63, coarse grinding, use W40 boron carbide / silicon carbide grinding paste to match the valve seat for coarse grinding, the grinding time is 2h-4h, until no grinding lines can be observed on the coating surface; different calibers and grinding speed configurations are shown in Table 1:

[0108] Table 1 Rough grinding grinding diameter and speed relationship

[0109]

[0110] S64, fine grinding, use W14 diamond grinding paste to grind with the matching valve seat manually on a rotating grinding platform, and compare every 10 minutes until the sealing surface roughness reaches 0.8;

[0111] When the sealing surface roughness reaches 0.8, use W3.5 diamond grinding paste for fine grinding, and compare every 10 minutes until the roughness reaches above 0.2; different calibers and grinding speed configurations are shown in Table 2:

[0112] Table 2 Relationship between grinding diameter and speed for fine grinding

[0113]

[0114] S65, polishing, use W0.5 diamond grinding paste to polish manually on a rotating grinding platform, compare every 10 minutes, and the product will be a mirror surface after polishing;

[0115] The configurations of different calibers and grinding speeds are shown in Table 3:

[0116] Table 3 Relationship between polishing and grinding diameter and rotation speed

[0117]

[0118] In this embodiment, the implementation of the above-mentioned grinding, lapping and polishing processes can effectively ensure the one-time qualified rate of the product, and the setting of constant parameters can effectively improve production efficiency, improve product quality stability, reduce production costs, and form standardized production.

[0119] S66. Leak detection. The method of leak detection is:

[0120] S661. Remove the grinding residue in kerosene and clean the ball 5 and the valve seat;

[0121] S662, fix the ball 5 so that the flow passage of the ball 5 remains parallel; place the valve seat on the ball 5 to ensure that the surrounding sealing surfaces fit tightly;

[0122] S663, penetration test: Pour kerosene into the valve seat flow channel and observe for 15 minutes. If there is no kerosene leakage, it is qualified; otherwise, repeat step S64 and pour kerosene again for observation;

[0123] S664, air blowing test: The contact area between the spherical surface of the ball 5 and the valve seat is tested with compressed air. If there is no bubble, it is qualified;

[0124] S665, flip the ball 5 180 degrees and fix it again, replace another valve seat and repeat steps S661 to S664;

[0125] S666. When the penetration test and blowing test of the corresponding spherical surfaces of the two valve seats are qualified, the inspection is completed and the grinding is qualified; the double leakage detection method of penetration test and blowing test can effectively prevent unqualified products from flowing into the next process and causing assembly rework, which can effectively improve the first-time qualified rate of assembly.

[0126] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "mounted / connected", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0127] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A supersonic spraying process for wear-resistant ball valve spheres. It is characterized in that A ball valve ball is subjected to supersonic spraying based on a wear-resistant ball valve ball spraying device, the wear-resistant ball valve ball spraying device comprising a base (1) and a spindle box (2) and a feeding mechanism respectively arranged on the base (1); The spindle box (2) is provided with a spindle (4) for driving the ball valve ball (5) to be processed to rotate; The feeding mechanism comprises a guide rail arranged on the base (1) and a feeding frame (3) movably connected to the guide rail; the feeding frame (3) is provided with a feeding rod (6) coaxially arranged with the main shaft (4) and used for inserting and fixing the ball (5); The base (1) is provided with a spraying component and a processing component respectively; the spraying component and the processing component both act on the sphere (5); The spraying assembly comprises a spraying device (7) and a spraying bracket for fixing the spraying device (7); the spraying bracket is movably connected to the base (1); The processing technology component comprises a plurality of flame nozzles (8), a plurality of cooling tubes (9) and a fixing bracket for fixing the flame nozzles (8) and the cooling tubes (9); the fixing bracket is movably connected to the base (1); The plurality of flame nozzles (8) and the plurality of cooling tubes (9) are arranged crosswise and at intervals; The distance between the spray head of the spraying device (7) and the sphere (5) is L , L 350mm-450mm; The spacing between adjacent flame nozzles (8) is M 1 , M 1 is 150mm-250mm; the distance between the flame nozzle (8) and the sphere (5) is M 2 , M 2 150mm-250mm; The supersonic spraying process of the wear-resistant ball valve ball comprises the following steps: S1, rough machining and surface treatment, and placing a sample block (10) on the sphere (5); S2, preheating, preheating the surface-treated sphere (5) to improve the bonding performance between the coating material and the surface of the sphere (5); S3, supersonic spraying, selecting a spraying material, and performing supersonic spraying on the sphere (5) through a spraying device (7); The method of supersonic spraying the sphere (5) by means of a spraying device (7) comprises the following steps: S31, select the spraying material as Cr3C2-25NiCr-SiC mixed powder with a particle size of 20μm-55μm; S32, clamp the ball (5) on the wear-resistant ball valve ball spraying device, and the interval from preheating to clamping completion shall not exceed 20 minutes; S33, adjusting the distance between the flame nozzle (8) and the outer circle of the sphere (5) so that the distance M2 between the flame nozzle (8) and the sphere (5) is 150 mm-250 mm; adjusting the flame nozzle (8) to the lower side opposite to the nozzle of the spraying device (7) and igniting it, and controlling the size of the spraying flame of the flame nozzle (8) to ensure that the surface temperature of the sphere (5) is uniform; S34, selecting a plurality of temperature interlayer measurement points (11) on the surface of the sphere (5) to measure the surface temperature of the sphere (5); when the surface temperature of the sphere (5) is between 80° C. and 100° C., starting supersonic spraying; When the surface temperature of the sphere (5) is greater than 150°C, spraying is stopped and cooling is performed through the cooling pipe (9); spraying is continued when cooling to 80°C-100°C; nitrogen gas at room temperature is introduced into the cooling pipe (9); S35, when the outer diameter of the sphere (5) is 0.8 mm larger than the size of the finished product drawing, the spraying is completed; S4, cooling treatment, removing the ball (5) from the wear-resistant ball valve ball spraying device and placing it in an insulation box for slow cooling treatment; S5, retaining the sample block (10), grinding the welding point position of the sample block (10) and removing the sample block (10) for bonding rate, porosity, hardness testing and keeping it for future reference; S6, a post-treatment process for the coating of the sphere (5), wherein the coating of the sphere (5) is sprayed and then treated to ensure the coating quality.

2. The supersonic spraying process for the wear-resistant ball valve ball according to claim 1, It is characterized in that The method for rough machining the sphere (5) in S1 is as follows: rough machining the sphere (5) into a forging blank, wherein the outer diameter is 0.8 mm smaller than the size of the finished part drawing; The method for arranging the sample blocks (10) on the sphere (5) in S1 is: spot welding the sample blocks (10) at the non-matching and sealing positions of the sphere (5), and the number of the sample blocks (10) is not less than 6; The method for surface treatment of the sphere (5) in S1 comprises the following steps: S11, cleaning the roughly machined sphere (5) with an environmentally friendly solvent-based cleaning agent to remove surface oil stains; S12, performing sandblasting on the surface of the rough-machined sphere (5), wherein the sandblasting material is white corundum sand, the particle size is 24-28 mesh, the sandblasting pressure is 0.6 MPa, the sandblasting distance is 100 mm, and the sandblasting moving speed is 200 mm / s-400 mm / s; S13. After the sandblasting is completed, a black light is used for inspection to ensure that there is no oil fluorescence in the sprayed area on the surface of the sphere (5).

3. The supersonic spraying process for the wear-resistant ball valve ball according to claim 1, It is characterized in that The method for preheating the surface-treated sphere (5) in S2 is: placing the sphere (5) in a heating box for preheating, raising the temperature to 110° C. to 130° C., and keeping the temperature for not less than 1 h / 25 mm; The interval between the surface treatment and preheating of the sphere (5) should not exceed 12 minutes to prevent contamination of the surface of the sphere (5).

4. The supersonic spraying process for the wear-resistant ball valve ball according to claim 1, It is characterized in that The method of selecting a plurality of temperature interlayer measurement points (11) in S34 is: setting them on a side close to the nozzle of the spraying device (7), and the number of the points set on the same horizontal line is not less than 3, and the number of the points set in the longitudinal direction is not less than 3 layers; When supersonic spraying is performed on the sphere (5) in S34, the relative running speed between the nozzle of the spraying device (7) and the sphere (5) is 450 mm / s-550 mm / s; the distance between the nozzle of the spraying device (7) and the sphere (5) is L It is 350mm-450mm; the fuel flow rate is 6.5GPH-7GPH; the oxygen flow rate is 1900SCFH-1950SCFH; the nitrogen flow rate is 25SCFH; and the powder feeding speed is 7r / min.

5. The supersonic spraying process for the wear-resistant ball valve ball according to claim 1, It is characterized in that In S4, the method for cooling the sprayed sphere (5) is: heat preservation and slow cooling, and the cooling time is 2h / 25mm.

6. The supersonic spraying process for the wear-resistant ball valve ball according to claim 1, It is characterized in that The post-coating treatment process of the sphere (5) in S6 comprises the following steps: S61, coating inspection; S62, grinding, using a spherical grinder to grind the outer circle of the sphere (5), the grinding size is the size of the fine part drawing, and the surface after grinding is uniform in metallic color without black skin or other spots; S63, coarse grinding, use W40 boron carbide / silicon carbide grinding paste to match the valve seat for coarse grinding, the grinding time is 2h-4h, until no grinding lines can be observed on the coating surface; S64, fine grinding, use W14 diamond grinding paste to grind with the matching valve seat manually on a rotating grinding platform, and compare every 10 minutes until the sealing surface roughness reaches 0.8; When the sealing surface roughness reaches 0.8, use W3.5 diamond grinding paste for fine grinding, and compare every 10 minutes until the roughness reaches above 0.2; S65, polishing, use W0.5 diamond grinding paste to polish manually on a rotating grinding platform, compare every 10 minutes, and the product will be a mirror surface after polishing; S66. Leak detection. The method of leak detection is: S661. Remove the grinding residue in kerosene and clean the ball (5) and valve seat; S662. Fix the sphere (5) so that the flow passages of the sphere (5) remain parallel; place the valve seat on the sphere (5) to ensure that the sealing surfaces on all sides fit tightly; S663, penetration test: Pour kerosene into the valve seat flow channel and observe for 15 minutes. If there is no kerosene leakage, it is qualified; otherwise, repeat step S64 and pour kerosene again for observation; S664, Air blowing test: The contact area between the ball surface (5) and the valve seat is tested with compressed air. If there are no bubbles, it is qualified. S665, flip the ball (5) 180 degrees and fix it again, replace another valve seat and repeat steps S661 to S664; S666. When the penetration test and blowing test of the corresponding spherical surfaces of the two valve seats are qualified, the inspection is completed and the grinding is qualified.

Citation Information

Cited By

  • Spraying device and spraying process for processing sphere of polycrystalline silicon spherical regulating valve

    CN119819519A

  • Spraying device and process for wear-resistant coating of ball body of titanium ball valve

    CN120900844A

  • A spraying device and process for a wear-resistant coating on a titanium ball valve ball.