Fluorescent perfluorinated acrylic coating material and preparation method thereof

The combination of fluorescent perfluoropolymer and silicone-modified styrene-acrylic emulsion solves the problem of insufficient performance and lack of fluorescent ability of acrylic coatings in high temperature and humid environments, achieving excellent waterproof, wear-resistant and Fluorescence properties expand the scope of applications.

CN118852933APending Publication Date: 2024-10-29SHENZHEN PAIQI NANO-TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410908494.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing acrylic electronic coatings have insufficient performance in high-temperature and humid environments and lack fluorescent capabilities, resulting in blurry or inaccurate displays of electronic instruments under low-light conditions. Waterproof and wear-resistant properties also need to be improved.

Method used

A combination of fluorescent perfluoropolymer, silicone-modified styrene-acrylic emulsion and fluorine solvent is used to prepare the fluorescent perfluoropolymer through the polymerization of carboxylic acid monomer, perfluoroalkylethylene and fluorene fluorine monomer, and combined with silicone-modified styrene-acrylic emulsion. It is compounded with styrene-acrylic emulsion to form a coating material with excellent waterproof, wear-resistant and fluorescent properties.

Benefits of technology

It significantly improves the hydrophobicity, high temperature resistance, acid and alkali resistance of the coating, and at the same time imparts fluorescent properties, enhances the mechanical properties and application range, and provides better waterproof and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0004932851000000021
    Figure BDA0004932851000000021
  • Figure BDA0004932851000000071
    Figure BDA0004932851000000071
Patent Text Reader

Abstract

The invention discloses a fluorescent perfluoropolymer coating material and a preparation method thereof. The fluorescent perfluoropolymer coating material comprises a fluorescent perfluoropolymer, an organic silicon modified styrene-acrylic emulsion and a fluorine solvent, the organic silicon modified styrene-acrylic emulsion is prepared by carrying out emulsion polymerization on methyl methacrylate, butyl acrylate, 3-trimethoxysilane propyl acrylate and styrene; the fluorescent perfluoropolymer is prepared by polymerizing a carboxylic acid monomer, perfluoroalkyl ethylene and a fluorene fluorine monomer. The fluorescent perfluoropolymer coating material disclosed by the invention is prepared by compounding the fluorescent perfluoropolymer, the organic silicon modified styrene-acrylic emulsion and the fluorine solvent, not only has the excellent waterproof capability of fluorine-containing acrylics, but also can further improve the wear resistance and the overall performance of a coating due to the addition of the organic silicon modified styrene-acrylic emulsion; and meanwhile, the coating material also has fluorescence capability, so that the application range of the formed coating can be expanded, and the coating material can be widely applied to the fields of electronic coatings and paints.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of fluorine-containing acrylic coatings, and in particular to a fluorescent perfluoropolymer coating material and a preparation method thereof. Background Art

[0002] As electronic products gradually turn to miniaturization, integration, and multifunctionality, the electronic assembly industry is also developing rapidly, and the requirements for the safety performance and appearance of assembled products are becoming higher and higher. After the electronic components are assembled, the circuit boards may be in different environments during use, such as humidity, smoke, chemical corrosion, high dust, vibration, etc., which may cause problems such as mildew and corrosion on the circuit boards, leading to circuit board failures.

[0003] Electronic coating is a specially formulated coating material with properties such as waterproof, moisture-proof, dust-proof, and resistance to cold and heat shock, aging, radiation, salt spray, ozone corrosion, vibration, good flexibility, and strong adhesion. Electronic coating is applied to the surface of the circuit board to form a transparent protective film. The protective film can protect the circuit board from damage in environments such as moisture, smoke, chemical corrosion, high dust, and vibration, thereby improving the reliability of the circuit board and the safety factor of the entire electronic component. This improves and extends their service life and ensures safety and reliability in use. Currently, it is increasingly used in printed circuit boards (PCBs), electrical equipment, semiconductors, sensors, transducers, and hybrid circuits.

[0004] At present, there are four main types of electronic coatings in China: epoxy resin, silicone, acrylate and polyurethane. Among them, acrylate coatings are cheap, transparent, flexible, and easy to repair, occupying a large market for electronic coatings. However, the high temperature resistance of acrylate electronic coatings is limited. Generally, it can only withstand high temperatures of about 130°C, and it tends to turn white in a humid environment. In addition, the surface energy of the film formed by acrylate coatings during coating is high, and it does not have water and oil repellency, resulting in poor water resistance, oil resistance and self-cleaning performance of the coating.

[0005] Therefore, the water resistance and other properties of acrylate can be improved by grafting or polymerizing fluorinated groups in acrylate. Fluorinated acrylate has the advantages of low surface tension, high mechanical strength, aging resistance, yellowing resistance, and good water resistance. Since the surface energy of its group -CF3 is only 6mJ / m 2 , giving it low surface free energy and water- and oil-repellent properties.

[0006] However, the fluorinated acrylate coatings in the prior art do not have fluorescent capabilities, which may cause electronic instruments to display blurry or inaccurate displays when the light brightness is insufficient, and the waterproof ability and wear resistance of the coating still need to be improved.

[0007] Therefore, there is an urgent need for a coating material with excellent waterproof and wear-resistant properties and fluorescent properties. Summary of the invention

[0008] Purpose of the invention: In view of the defects of the prior art, the purpose of the present invention is to provide a fluorescent perfluoropolymer coating material with excellent waterproof ability and wear resistance and fluorescent properties and a preparation method thereof.

[0009] Technical solution:

[0010] A fluorescent perfluoropolymer coating material, comprising a fluorescent perfluoropolymer, an organosilicon-modified styrene-acrylic emulsion and a fluorine-based solvent;

[0011] The organosilicon-modified styrene-acrylic emulsion is prepared by emulsion polymerization of methyl methacrylate, butyl acrylate, 3-trimethoxysilane propyl acrylate and styrene;

[0012] The fluorescent perfluoropolymer is prepared by polymerizing carboxylic acid monomers, perfluoroalkylethylene and fluorene fluoride monomers;

[0013] The fluorene fluoride monomer has a structure as shown in the following formula A:

[0014]

[0015] Furthermore, the carboxylic acid monomer is selected from one of acrylic acid, methacrylic acid or 2-butenoic acid; and the perfluoroalkylethylene is selected from one of perfluorobutylethylene, perfluorohexylethylene, perfluorodecylethylene or perfluorododecylethylene.

[0016] Furthermore, the fluorescent perfluoropolymer is prepared by the following steps: in a reactor, carboxylic acid monomer, perfluoroalkylethylene and fluorene fluoride monomer are added in proportion, stirred evenly and then heated to 60-80°C, an initiator is added, stirred for reaction for 2-3 hours, and then cooled, filtered, washed and dried to obtain the fluorescent perfluoropolymer.

[0017] The fluorescent perfluoropolymer of the present invention has perfluoroalkylethylene polymerized in its structure. Based on the lower surface energy of the carbon-fluorine bond, the surface activity of the polymer can be significantly improved, thereby improving the hydrophobicity of the prepared coating. The excellent stability of the carbon-fluorine bond can improve the high temperature resistance and acid and alkali resistance of the polymer, so that the prepared coating has excellent weather resistance. Based on the coplanarity, rigidity and larger conjugated system of the fluorene ring structure, electrons can be easily excited, thereby giving the polymer excellent fluorescent properties and expanding the application range of the prepared coating. At the same time, based on the strong rigidity of the fluorene ring structure and the lower surface energy of the carbon-fluorine bond, not only the surface activity of the polymer can be further improved, but also the mechanical properties of the prepared coating can be enhanced, thereby improving its wear resistance.

[0018] Furthermore, the molar ratio of the carboxylic acid monomer, the perfluoroalkylethylene and the fluorene fluoride monomer is (15-25): (5-8): (3-5).

[0019] Furthermore, the fluorine-based solvent is selected from one of hydrochlorofluorocarbons, hydrofluorocarbons, perfluorocarbons, perfluoroethers or hydrofluoroethers.

[0020] Furthermore, the organosilicon-modified styrene-acrylic emulsion is prepared by the following steps:

[0021] (1) Add emulsifier, methyl methacrylate, butyl acrylate and deionized water into a reactor, stir evenly, heat to 50-60°C, keep warm for 10-20 minutes, then heat to 70-80°C, add initiator, keep warm for 1-2 hours, then cool to 40-50°C;

[0022] (2) Add 3-trimethoxysilane acrylate, styrene and initiator to the reactor of step (1), stir evenly, keep warm for reaction for 12-18 hours, then raise the temperature to 80-90° C., add emulsifier, keep warm for reaction for 2-3 hours, and cool to obtain the organosilicon-modified styrene-acrylic emulsion.

[0023] The organosilicon-modified styrene-acrylic emulsion of the present invention can improve the thermal stability of the styrene-acrylic emulsion by grafting 3-trimethoxysilane propyl acrylate, and its silane structure can be cross-linked to form a network structure in the prepared coating, further improving the wear resistance and waterproof ability of the coating, and its propyl acrylate structure can improve the compatibility of the styrene-acrylic emulsion and the fluorescent perfluoropolymer, so that the two can be evenly compounded to form a stable coating material.

[0024] Furthermore, the emulsifier is selected from one of sodium dodecylbenzene sulfonate, sodium octyl acrylate or sodium dodecyl polyoxyethylene ether sulfate; and the initiator is selected from one of ammonium persulfate or azobisisobutyronitrile.

[0025] Furthermore, the molar ratio of methyl methacrylate, butyl acrylate, 3-trimethoxysilane propyl acrylate and styrene is (10-15): (5-10): (5-8): (15-20).

[0026] The preparation method of any one of the above fluorescent perfluoropolymer coating materials comprises the following steps: adding a fluorescent perfluoropolymer and a fluorine-based solvent into a reactor, stirring evenly and heating to 40-50°C, adding a silicone-modified styrene-acrylic emulsion, stirring at 600-800 r / min for 20-30 minutes and then cooling to obtain the fluorescent perfluoropolymer coating material.

[0027] The organosilicon-modified styrene-acrylic emulsion and the fluorescent perfluoropolymer in the present invention have a certain synergistic effect in the material structure, which can make up for the pores existing in the single-component coating. In addition, based on the advantages of the styrene-acrylic emulsion in water resistance, corrosion resistance, aging resistance and high mechanical properties, the composite organosilicon-modified styrene-acrylic emulsion in the coating material can effectively improve the waterproof ability and wear resistance of the coating material.

[0028] Furthermore, the mass ratio of the fluorescent perfluoropolymer, the silicone-modified styrene-acrylic emulsion and the fluorine-based solvent is (20-30):(5-8):(50-70).

[0029] Beneficial effects:

[0030] (1) The fluorescent perfluoropolymer coating material provided by the present invention is prepared by compounding a fluorescent perfluoropolymer, an organosilicon-modified styrene-acrylic emulsion and a fluorine-based solvent. It not only has the excellent waterproof ability of fluorinated acrylates, but the addition of the organosilicon-modified styrene-acrylic emulsion can further improve the wear resistance and overall performance of the coating. At the same time, the coating material also has fluorescent ability, which can expand the application range of the coating, so that it can be widely used in the fields of electronic coatings and paints.

[0031] (2) The fluorescent perfluoropolymer in the fluorescent perfluoropolymer coating material provided by the present invention has perfluoroalkylethylene polymerized in its structure. Based on the lower surface energy of the carbon-fluorine bond, the surface activity of the polymer can be significantly improved, thereby improving the hydrophobicity of the coating. The excellent stability of the carbon-fluorine bond can improve the high temperature resistance and acid and alkali resistance of the polymer, so that the coating has excellent weather resistance. Based on the coplanarity, rigidity and larger conjugated system of the fluorene ring structure, electrons can be easily excited, thereby giving the polymer excellent fluorescent properties and expanding the application range of the coating. At the same time, based on the strong rigidity of the fluorene ring structure and the lower surface energy of the carbon-fluorine bond, not only can the surface activity of the polymer be further improved, but also the mechanical properties of the coating can be enhanced, thereby improving its wear resistance.

[0032] (3) In the fluorescent perfluoropolymer coating material provided by the present invention, the organosilicon-modified styrene-acrylic emulsion and the fluorescent perfluoropolymer have a certain synergistic effect in the material structure, which can make up for the pores existing in the single-component coating. In addition, based on the advantages of styrene-acrylic emulsion such as water resistance, corrosion resistance, aging resistance and high mechanical properties, the composite organosilicon-modified styrene-acrylic emulsion in the coating material can effectively improve the waterproof ability and wear resistance of the coating material.

[0033] (4) The organosilicon-modified styrene-acrylic emulsion in the fluorescent perfluoropolymer coating material provided by the present invention can improve the thermal stability of the styrene-acrylic emulsion by grafting 3-trimethoxysilane propyl acrylate, and its silane structure can cross-link with each other in the prepared coating to form a network structure, further improving the wear resistance and waterproof ability of the coating, and its propyl acrylate structure can improve the compatibility of the styrene-acrylic emulsion and the fluorescent perfluoropolymer, so that the two can be evenly compounded to form a stable coating material. DETAILED DESCRIPTION

[0034] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0035] The commercially available styrene acrylic emulsion was purchased from Zhengzhou Wandao New Material Technology Co., Ltd.; the commercially available waterproof coating paint was RJ anti-ozone anti-corrosion waterproof coating purchased from Guangdong Huolun Building Materials Technology Development Co., Ltd.; the remaining reagents and equipment were conventional reagents and equipment in this technical field.

[0036] Preparation of Fluorene Fluoride Monomer

[0037] Fluorene fluoride monomer was prepared by the following steps:

[0038] In a reactor, 50 mL of N,N-dimethylacetamide, 0.02 mol of 9-fluorene methanol and 0.3 g of potassium carbonate were added, heated to 45° C. and stirred to dissolve, 0.03 mol of 4-bromo-3,3,4,4-tetrafluorobutene was slowly added dropwise, and after the addition was completed, the mixture was kept warm for reaction for 50 minutes, then cooled, filtered, washed and dried to obtain the fluorene fluoride monomer;

[0039] Mass spectrum data of fluorene fluoride monomer: The product was analyzed by LC-MS, and the m / z of the product was 322.10 (100.0%), 323.11 (19.8%), and 324.11 (1.9%).

[0040] Preparation of fluorescent perfluoropolymer

[0041] The fluorescent perfluoropolymer for coating was prepared by the following steps:

[0042] In the reactor, add 0.15 mol of acrylic acid, 0.05 mol of perfluorobutylethylene and 0.03 mol of fluorene fluoride monomer, stir evenly, heat to 70°C, add 0.3 g of azobisisobutyronitrile, stir and react for 3 hours, then cool, filter, wash and dry to obtain the fluorescent perfluoropolymer for coating.

[0043] Preparation of silicone modified styrene acrylic emulsion-1

[0044] The silicone-modified styrene-acrylic emulsion-1 was prepared by the following steps:

[0045] (1) In a reactor, add 0.3 g of sodium dodecylbenzene sulfonate, 0.05 mol of methyl methacrylate, 0.03 mol of butyl acrylate and 150 mL of deionized water, stir evenly and heat to 60° C., keep warm for 20 minutes and then heat to 75° C., add 0.1 g of ammonium persulfate and keep warm for 2 hours and then cool to 45° C.;

[0046] (2) Add 0.03 mol of 3-trimethoxysilane acrylate, 0.1 mol of styrene and 0.2 g of azobisisobutyronitrile to the reactor of step (1), stir evenly, keep warm for reaction for 18 hours, then raise the temperature to 90° C., add 0.3 g of sodium dodecylbenzene sulfonate, keep warm for reaction for 3 hours, and cool to obtain the organosilicon-modified styrene-acrylic emulsion-1.

[0047] Preparation of silicone modified styrene acrylic emulsion-2

[0048] The preparation method is basically the same as that of silicone modified styrene acrylic emulsion-1, except that 3-trimethoxysilane propyl acrylate is replaced by an equal amount of vinyl trimethoxysilane.

[0049] Example 1

[0050] The fluorescent perfluoropolymer coating material was prepared by the following steps:

[0051] In the reactor, 25 g of fluorescent perfluoropolymer and 70 g of perfluorododecane were added, stirred evenly and then heated to 45° C., 5 g of silicone-modified styrene-acrylic emulsion-1 was added, stirred at 800 r / min for 30 minutes and then cooled to obtain the fluorescent perfluoropolymer coating material.

[0052] Example 2

[0053] The method is basically the same as Example 1, except that the components and their masses are changed to 30 g of fluorescent perfluoropolymer, 60 g of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether and 7 g of silicone-modified styrene acrylic emulsion-1.

[0054] Example 3

[0055] The method is basically the same as Example 1, except that the components and their masses are changed to 20 g of fluorescent perfluoropolymer, 50 g of pentafluoropropanol and 8 g of silicone-modified styrene-acrylic emulsion-1.

[0056] Comparative Example 1

[0057] Commercially available waterproof coating paint.

[0058] Comparative Example 2

[0059] The method is basically the same as Example 1, except that the fluorescent perfluoropolymer is replaced by an equal amount of perfluoroalkylethyl acrylate.

[0060] Comparative Example 3

[0061] The method is basically the same as Example 1, except that the silicone-modified styrene-acrylic emulsion-1 is replaced by an equal amount of perfluorododecane.

[0062] Comparative Example 4

[0063] The method is basically the same as Example 1, except that the silicone-modified styrene-acrylic emulsion-1 is replaced by an equal amount of commercially available styrene-acrylic emulsion.

[0064] Comparative Example 5

[0065] The method is basically the same as Example 1, except that the organosilicon-modified styrene-acrylic emulsion-1 is replaced by an equal amount of organosilicon-modified styrene-acrylic emulsion-2.

[0066] Performance Testing

[0067] According to the standard of GB / T19250-2003, the products of Examples 1-3 and Comparative Examples 1-5 were made into paint films, and performance tests were performed after drying for 7 days.

[0068] Fluorescence performance detection: The fluorescence intensity and fluorescence color of the paint films made from the products of Examples 1-3 and Comparative Examples 1-5 were detected at 310 nm.

[0069] Waterproof ability test: According to the test standard of GB / T19250-2003, the water impermeability of the paint films made from the products of Examples 1-3 and Comparative Examples 1-5 was tested under the conditions of 0.3 MPa and 30 min.

[0070] Wear resistance test: According to the test standard of GB / T 1768-2006 "Determination of wear resistance of paints and varnishes - Rotating rubber grinding wheel method", the paint films made from the products of Examples 1-3 and Comparative Examples 1-5 were tested for the wear quality of the same specifications under the condition of 750g / 500r.

[0071] The test results are shown in the following table:

[0072]

[0073] According to the comparison of the test results of Examples 1-3 with those of Comparative Example 1, it can be seen that the fluorescent perfluoropolymer coating material provided by the present invention has excellent waterproof performance and fluorescence, and has stronger wear resistance than the coating materials in the prior art, and can be widely used in the field of electronic coatings and paints.

[0074] According to the comparison of the test results of Examples 1-3 and Comparative Example 2, adding fluorescent perfluoropolymer to the fluorescent perfluoropolymer coating material provided by the present invention can give the coating material fluorescence and improve the waterproof ability and wear resistance of the coating.

[0075] According to the comparison of the test results of Examples 1-3 and Comparative Examples 3-5, it can be seen that the fluorescent perfluoropolymer coating material provided by the present invention contains an organosilicon-modified styrene-acrylic emulsion, which has excellent compatibility with the fluorescent perfluoropolymer and can significantly improve the wear resistance and waterproof ability of the coating.

[0076] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A fluorescent perfluoropolymer coating material, characterized in that: Contains fluorescent perfluoropolymer, silicone-modified styrene-acrylic emulsion and fluorinated solvent; The organosilicon-modified styrene-acrylic emulsion is prepared by emulsion polymerization of methyl methacrylate, butyl acrylate, 3-trimethoxysilane propyl acrylate and styrene; The fluorescent perfluoropolymer is prepared by polymerizing carboxylic acid monomers, perfluoroalkylethylene and fluorene fluoride monomers; The fluorene fluoride monomer has a structure as shown in the following formula A: 。 2. The fluorescent perfluoropolymer coating material according to claim 1, characterized in that: The carboxylic acid monomer is selected from one of acrylic acid, methacrylic acid or 2-butenoic acid; the perfluoroalkylethylene is selected from one of perfluorobutylethylene, perfluorohexylethylene, perfluorodecylethylene or perfluorododecylethylene.

3. The fluorescent perfluoropolymer coating material according to claim 1, characterized in that: The fluorescent perfluoropolymer is prepared by the following steps: in a reactor, carboxylic acid monomer, perfluoroalkylethylene and fluorene fluoride monomer are added in proportion, stirred evenly and then heated to 60-80° C., an initiator is added, stirred for reaction for 2-3 hours, and then cooled, filtered, washed and dried to obtain the fluorescent perfluoropolymer.

4. The fluorescent perfluoropolymer coating material according to claim 3, characterized in that: The molar ratio of the carboxylic acid monomer, the perfluoroalkylethylene and the fluorene fluoride monomer is (15-25): (5-8): (3-5).

5. The fluorescent perfluoropolymer coating material according to claim 1, characterized in that: The fluorine-based solvent is selected from one of hydrochlorofluorocarbons, hydrofluorocarbons, perfluorocarbons, perfluoroethers or hydrofluoroethers.

6. The fluorescent perfluoropolymer coating material according to claim 1, characterized in that: The organosilicon-modified styrene-acrylic emulsion is prepared by the following steps: (1) Add emulsifier, methyl methacrylate, butyl acrylate and deionized water into the reactor, stir evenly and heat to 50-60°C, keep the temperature for 10-20 minutes and then heat to 70-80°C, add initiator and keep the temperature for 1-2 hours and then cool to 40-50°C; (2) Add 3-trimethoxysilane acrylate, styrene and initiator to the reactor of step (1), stir evenly, keep warm for reaction for 12-18 hours, then raise the temperature to 80-90° C., add emulsifier, keep warm for reaction for 2-3 hours, and cool to obtain the organosilicon-modified styrene-acrylic emulsion.

7. The fluorescent perfluoropolymer coating material according to claim 6, characterized in that: The emulsifier is selected from one of sodium dodecylbenzene sulfonate, sodium octyl acrylate or sodium dodecyl polyoxyethylene ether sulfate; the initiator is selected from one of ammonium persulfate or azobisisobutyronitrile.

8. The fluorescent perfluoropolymer coating material according to claim 6, characterized in that: The molar ratio of methyl methacrylate, butyl acrylate, 3-trimethoxysilane propyl acrylate and styrene is (10-15): (5-10): (5-8): (15-20).

9. The method for preparing the fluorescent perfluoropolymer coating material according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: adding a fluorescent perfluoropolymer and a fluorine solvent into a reactor, stirring evenly and heating to 40-50°C, adding an organosilicon-modified styrene-acrylic emulsion, stirring at 600-800 r / min for 20-30 minutes and then cooling to obtain the fluorescent perfluoropolymer coating material.

10. The method for preparing the fluorescent perfluoropolymer coating material according to claim 9, characterized in that: The mass ratio of the fluorescent perfluoropolymer, the silicone-modified styrene-acrylic emulsion and the fluorine-based solvent is (20-30): (5-8): (50-70).