Efficient green chemical mechanical polishing solution based on phytic acid-phytate as well as preparation method and polishing method of efficient green chemical mechanical polishing solution

By using phytic acid-phytates in green chemical mechanical polishing fluids, the problem of reduced oxidation capacity caused by the reaction of organic acids and oxidants is solved, achieving more efficient polishing effects and stronger anti-corrosion capabilities, and simplifying the components of the polishing fluid. structure and reduce environmental impact.

CN118852986APending Publication Date: 2024-10-29HANGZHOU DIANZI UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410848324.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

When organic acids and amino acids in existing green chemical mechanical polishing fluids react with oxidants, their oxidation capabilities are reduced and their corrosion inhibition capabilities are weakened, causing problems such as pitting corrosion and excessive metal ions.

Method used

Phytic acid - phytate is used as a green organic acid and corrosion inhibitor. It adjusts pH through its multiple functions, acts as a corrosion inhibitor and complexing agent, avoids reaction with oxidants, reduces free metals, and improves the oxidation ability and service life of the polishing fluid. .

Benefits of technology

It improves the oxidation ability and service life of the polishing fluid, reduces pitting corrosion defects and excessive metal ions, enhances polishing quality and anti-corrosion capabilities, simplifies the component structure of the polishing fluid and reduces negative environmental impacts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852986A_ABST
    Figure CN118852986A_ABST
Patent Text Reader

Abstract

The invention discloses an efficient green chemical mechanical polishing solution based on phytic acid-phytate as well as a preparation method and a polishing method of the efficient green chemical mechanical polishing solution. The polishing solution comprises the following components in percentage by weight: 0.01 wt%-0.2 wt% of phytic acid, 0.1 wt%-1 wt% of phytate, 0.5 wt%-3 wt% of H2O2, 10 wt%-30 wt% of an abrasive and the balance of deionized water. The phytic acid-phytate with multiple effects is added into the polishing solution, so that the pH can be adjusted, the phytic acid-phytate can serve as a corrosion inhibitor and a complexing agent, the component structure of the polishing solution can be effectively simplified, the pitting corrosion defect is reduced, free metal in the polishing solution is reduced, and the corrosion resistance of polished metal is improved. Meanwhile, phytic acid-phytate cannot react with hydrogen peroxide, so that the service life of the polishing solution can be effectively prolonged, and the oxidation capacity of the polishing solution can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical mechanical polishing, and more specifically to a high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate, a preparation method thereof and a polishing method. Background Art

[0002] Chemical mechanical polishing (CMP) is widely used in fine processing of various metal surfaces. TC4 titanium alloy has good comprehensive mechanical properties and has been widely used in various industrial fields. However, titanium alloy has disadvantages such as high friction coefficient, poor corrosion resistance and poor wear resistance, which seriously restricts its application. Therefore, it is extremely important to improve the comprehensive performance of TC4 titanium alloy through surface polishing.

[0003] Polishing fluid is an important component of CMP and has a decisive influence on polishing removal rate and surface roughness. In recent years, in response to environmental protection needs, CMP polishing fluid has gradually developed in the direction of green environmental protection, and toxic and harmful components in CMP have gradually been replaced by non-toxic and biocompatible components. For example, hydrogen peroxide is used as an oxidant to replace traditional nitric acid, persulfate, etc.; organic acids (acetic acid, malic acid, citric acid, tartaric acid, etc.) are used to replace hydrochloric acid, phosphoric acid, sulfuric acid, etc. in metal polishing fluid; amino acids (such as glycine) are used to replace toxic corrosion inhibitors and chelating agents in metal polishing fluids.

[0004] However, there are still some problems in the new green chemical mechanical polishing liquid: first, the organic acids and amino acids currently used have certain reducing properties. When preparing the polishing liquid, they will undergo redox reactions with the oxidant-hydrogen peroxide, resulting in a decrease in the oxidizing ability of the polishing liquid, which ultimately affects the polishing performance; at the same time, the oxidized organic acids and amino acids will also cause problems such as a decrease in the corrosion inhibition ability and chelating ability of the polishing liquid, leading to pitting corrosion and excessive metal ions in the polishing liquid. Summary of the invention

[0005] The purpose of the present invention is to overcome the above-mentioned defects of the prior art, and to provide a high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate, a preparation method thereof, and a polishing method thereof. The present invention not only adjusts the pH value, but also acts as a corrosion inhibitor and a complexing agent by adding phytic acid-phytate with multiple functions to the polishing liquid, and can effectively simplify the polishing liquid component structure, reduce pitting defects, reduce free metals in the polishing liquid, and improve the anti-corrosion ability of the metal after polishing. At the same time, phytic acid-phytate will not react with hydrogen peroxide, and can effectively improve the service life and oxidation ability of the polishing liquid.

[0006] To achieve the above object, the technical solution of the present invention is as follows:

[0007] A high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate comprises the following components in weight percentage: 0.01wt%-0.2wt% of phytic acid, 0.1wt%-1wt% of phytate, 0.5wt%-3wt% of H2O2, 10wt%-30wt% of abrasive and the balance is deionized water.

[0008] The present invention also discloses a method for preparing the above-mentioned efficient green chemical mechanical polishing liquid based on phytic acid-phytate, comprising the following steps: mixing phytic acid, phytate, abrasive, H2O2 and deionized water to obtain the polishing liquid.

[0009] The present invention also discloses a high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate as described above, or a polishing method for the high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate prepared by the above-mentioned preparation method, comprising: injecting the polishing liquid between the polishing pad and the TC4 titanium alloy at room temperature, performing chemical mechanical polishing on the TC4 titanium alloy, and cleaning and drying after polishing to obtain the polished TC4 titanium alloy.

[0010] Implementing the embodiments of the present invention will have the following beneficial effects:

[0011] 1. The present invention provides a high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate, wherein phytic acid is a saturated green organic acid, which will not pollute the environment, is not reducing, and will not undergo redox reaction with hydrogen peroxide, thereby effectively improving the service life and oxidation capacity of the polishing liquid, and solving the problem that both organic acids and amino acids in traditional green polishing liquids can reduce hydrogen peroxide, causing the performance of the polishing liquid to decline.

[0012] 2. The efficient green chemical mechanical polishing liquid based on phytic acid-phytate provided by the present invention, phytate has a strong coordination and chelating ability, and can form a stable complex with a variety of metals and ions through van der Waals action, electrostatic action, and coordination bond action, thereby acting as a corrosion inhibitor and chelating agent. As a corrosion inhibitor, it can weaken the excessive erosion of protons on metals, thereby reducing pitting defects and improving polishing quality. As a complexing agent, free metal ions in the polishing liquid can be captured to form insoluble precipitation, and separated by centrifugation / precipitation in one step, thereby reducing the negative impact of the polishing liquid on the environment.

[0013] 3. The high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate provided by the present invention, wherein the phytic acid-phytate can be used as a pH buffer pair to stabilize the acidity and alkalinity of the polishing liquid, and will not cause pH fluctuations due to the consumption of hydrogen ions during the polishing process, thereby ensuring the consistency of the performance of the polishing liquid.

[0014] 4. The high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate provided by the present invention, phytic acid-phytate can act as a dispersant to a certain extent, stabilize the abrasive, and reduce the agglomeration of the abrasive.

[0015] 5. The efficient and green chemical mechanical polishing liquid based on phytic acid-phytate provided by the present invention can greatly simplify the component structure and preparation process of the polishing liquid and reduce the preparation cost of the polishing liquid due to the multi-effects of phytic acid-phytate.

[0016] 6. The high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate provided by the present invention, after polishing the metal sample, the phytic acid-phytate therein will partially adhere to the polished metal surface, play an anti-corrosion role, thereby increasing the service life of the metal. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 is the chemical structural formula of oxalic acid of the present invention.

[0018] Figure 2 This is a surface morphology image of the polished titanium alloy sample of Example 2 of the present invention.

[0019] Figure 3 This is a surface morphology image of the polished titanium alloy sample of Example 5 of the present invention.

[0020] Figure 4 This is a surface morphology diagram of the polished titanium alloy sample of Comparative Example 1 of the present invention.

[0021] Figure 5 This is a surface morphology of the polished titanium alloy sample of Comparative Example 2 of the present invention.

[0022] Figure 6 This is a surface morphology of the polished titanium alloy sample of Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0023] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited in any way.

[0024] The inventors have found that phytic acid is a saturated organic acid with a structural formula as follows: Figure 1 As shown, it is widely found in plants and can be used in the fields of food and cosmetics processing. It is harmless to the human body and the environment. At the same time, deprotonated phytic acid has a strong coordination and chelating ability. It can form stable complexes with a variety of metals and ions through van der Waals action, electrostatic action, and coordination bond action, thereby acting as a corrosion inhibitor and complexing agent.

[0025] The present invention obtained based on these findings is as follows.

[0026] The invention discloses a high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate, which comprises the following components in weight percentage: 0.01wt%-0.2wt% of phytic acid, 0.1wt%-1wt% of phytate, 0.5wt%-3wt% of H2O2, 10wt%-30wt% of abrasive and the balance is deionized water.

[0027] The polishing liquid provided by the present invention has multiple functions by adding phytic acid-phytate, specifically: phytic acid, as a saturated green organic acid, has no reducing property, so it will not undergo redox reaction with hydrogen peroxide, thereby avoiding reducing the oxidizing property of the polishing liquid, and solving the problem that organic acids (such as malic acid, citric acid, tartaric acid, etc.) and amino acids in traditional green polishing liquids can reduce hydrogen peroxide, causing the performance of the polishing liquid to decline. At the same time, the present invention adds phytate with strong coordination and chelating ability, which can form a stable complex with various metals and ions through van der Waals action, electrostatic action, and coordination bond action, thereby acting as a corrosion inhibitor and complexing agent; as a corrosion inhibitor, it can weaken the excessive erosion of protons on metals, thereby reducing pitting defects and improving polishing quality; as a complexing agent, it can capture free metal ions in the polishing liquid to form insoluble precipitation, and separate by centrifugation / precipitation in one step, thereby reducing the negative impact of the polishing liquid on the environment. At the same time, phytic acid-phytate can also act as a pH buffer pair to stabilize the acidity and alkalinity of the polishing liquid, and will not cause pH fluctuations due to the consumption of hydrogen ions during the polishing process, thereby ensuring the consistency of the polishing liquid performance.

[0028] In one embodiment, the pH of the polishing liquid is 2-5.

[0029] In a specific embodiment, the phytate includes one or both of sodium phytate and potassium phytate.

[0030] In a specific embodiment, the abrasive includes one or both of spherical SiO2 and spherical Al2O3.

[0031] In a specific embodiment, the particle size of the abrasive is 20 nm to 500 nm.

[0032] In a specific embodiment, when the abrasive is spherical SiO2, its particle size is preferably 20nm-300nm.

[0033] In a specific embodiment, when the abrasive is spherical Al2O3, its particle size is preferably 50nm-500nm.

[0034] The present invention also discloses a method for preparing a high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate as in any embodiment of the present invention, comprising the following steps: mixing phytic acid, phytate, abrasive, H2O2 and deionized water to obtain a polishing liquid.

[0035] In a specific embodiment, the preparation method specifically includes: mixing phytic acid, phytate and deionized water and stirring for 10 minutes to 30 minutes, adding abrasive to the obtained mixed solution, ultrasonicating for 30 minutes to 60 minutes at room temperature, and then stirring for 4 hours to 6 hours, adding H2O2 to the suspension in which the abrasive is fully dispersed, and continuing to stir for 2 minutes to 5 minutes to obtain the corresponding polishing liquid, and storing it at room temperature away from light.

[0036] Specifically, phytic acid-phytate can also act as a dispersant to a certain extent, stabilize the abrasive and reduce agglomeration of the abrasive.

[0037] The present invention also discloses a high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate as in any embodiment of the present invention, or a polishing method for a high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate prepared by the preparation method of any embodiment of the present invention, comprising: injecting the polishing liquid between the polishing pad and the TC4 titanium alloy at room temperature, performing chemical mechanical polishing on the TC4 titanium alloy, and cleaning and drying after the polishing to obtain the polished TC4 titanium alloy.

[0038] Specifically, after the metal sample is polished, the phytic acid-phytate in the polishing liquid will partially adhere to the polished metal surface to play an anti-corrosion role, thereby increasing the service life of the metal.

[0039] In a specific embodiment, during the chemical mechanical polishing process, the rotation speed of the polishing pad is controlled to be 100rpm to 500rpm; the flow rate of the polishing liquid is 2mL / min to 5mL / min; the polishing pressure is 5MPa to 20MPa; and the polishing time is 30min to 120min.

[0040] In one specific embodiment, the polishing pad is made of polyurethane.

[0041] The following are specific embodiments

[0042] The component ratios of the polishing liquids of Examples 1-6 of the present invention and Comparative Examples 1-3 are shown in Table 1.

[0043]

[0044]

[0045] In Table 1, “+” represents pitting defects, and the more pitting defects there are, the more pitting defects there are; “*” represents corrosion resistance, and the more pitting defects there are, the stronger the corrosion resistance is.

[0046] Test Case

[0047] 1. Polishing experiments were conducted on the polishing liquids of Examples 1-6 and Comparative Examples 1-3. Specifically, the polishing sample was TC4 titanium alloy with a size of 1cm*1cm. The TC4 titanium alloy sample was fixed on a UNIPOL-1200S chemical mechanical polishing device, polyurethane was used as the polishing pad, the polishing pressure was set to 40MPa, and the speed was set to 300rpm. At room temperature, the above-mentioned polishing liquid was continuously stirred on the agitator for 10 minutes, and the peristaltic pump was turned on to continuously inject the polishing liquid into the polishing device at a flow rate of 2mL / min, and polishing was performed for 60 minutes. After polishing, the TC4 titanium alloy sample was removed, thoroughly washed with deionized water, and blown dry.

[0048] Polishing removal rate and roughness test: The surface pitting defects of the polished sample were roughly observed by metallographic microscope, and the surface roughness Ra of the polished sample was analyzed by ZygoNewView9000 white light interferometer. The polishing removal rate Rr was characterized by weighing method, which can be calculated by the mass difference of the sample before and after polishing. Let the mass of the sample before polishing be m1, the mass of the sample after polishing be m2, the area of ​​the polished sample be S, and the density be p, then:

[0049]

[0050] Corrosion resistance test: The polished sample was immersed in a 1wt% sodium chloride aqueous solution, and its corrosion potential was tested by an electrochemical workstation, using a three-electrode system: platinum mesh as the counter electrode, Ag / AgCl as the reference electrode, and a scanning speed of 1mv / s. The larger the corrosion potential, the stronger its corrosion resistance.

[0051] According to the test results in Table 1, after phytic acid-phytate is introduced into the polishing liquid of Examples 1-6, the polishing efficiency and polishing quality of Examples 1-6 are better than those of Comparative Examples 1-3, indicating that phytic acid and phytate have a synergistic effect on the polishing effect.

[0052] According to the test results of Comparative Example 2 and Example 5 in Table 1, when phytate is not added, the pitting defects of Comparative Example 2 are not effectively controlled compared with Example 5, which shows that phytate is a key component for controlling pitting corrosion, which can be used as a corrosion inhibitor to weaken the excessive corrosion of protons on metals, thereby reducing pitting defects and improving polishing quality.

[0053] It can be seen from Comparative Example 3 and Example 2, and with reference to Figure 2 and Figure 6 The polishing liquid with malic acid added has the most serious pitting defects, and the polishing effect of titanium alloy is poor due to the reaction and consumption of malic acid and hydrogen peroxide. This shows that by adding phytic acid, no redox reaction will occur with hydrogen peroxide, thereby not reducing the oxidizing performance of the polishing liquid.

[0054] It can be seen from Comparative Examples 1-2 and Examples 2 and 5, and with reference to Figure 2-Figure 5 The surface morphology of the polished titanium alloy sample shown in the figure shows that when only phytate or only phytic acid is added, the surface roughness and removal rate are significantly attenuated, indicating that phytic acid and phytate have a synergistic effect on pH regulation, indicating that phytic acid-phytate can also be used as a pH buffer pair to stabilize the acidity and alkalinity of the polishing solution, and will not cause pH fluctuations due to the consumption of hydrogen ions during the polishing process, thereby ensuring the consistency of the polishing solution performance.

[0055] According to the test data in Table 1, after phytic acid-phytate is introduced into the polishing liquid of Examples 1-6, the corrosion resistance of Examples 1-6 is better than that of Comparative Examples 1-3, indicating that phytic acid and phytate have a synergistic effect on the anti-corrosion effect and can effectively improve the corrosion resistance of polished titanium alloy.

[0056] In summary, the phytic acid-phytate in the polishing liquid of the embodiment of the present invention has multiple functions, not only can it adjust the pH, but also can act as a corrosion inhibitor and a complexing agent, which can effectively simplify the component structure of the polishing liquid, reduce pitting defects, reduce free metals in the polishing liquid, and improve the anti-corrosion ability of the metal after polishing. At the same time, phytic acid-phytate will not react with hydrogen peroxide, which can effectively improve the service life and oxidation ability of the polishing liquid, and can be applied to the polishing field of various metals.

[0057] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A highly efficient green chemical mechanical polishing liquid based on phytic acid-phytate, characterized in that: The composition includes the following weight percentages: 0.01wt% to 0.2wt% of phytic acid, 0.1wt% to 1wt% of phytate, 0.5wt% to 3wt% of H2O2, 10wt% to 30wt% of abrasive and the balance is deionized water.

2. The high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate according to claim 1, characterized in that: The pH value of the polishing liquid is 2-5.

3. The efficient green chemical mechanical polishing liquid based on phytic acid-phytate according to claim 1, characterized in that: The phytate includes one or both of sodium phytate and potassium phytate.

4. The high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate according to claim 1, characterized in that: The abrasive includes one or both of spherical SiO2 and spherical Al2O3.

5. The efficient green chemical mechanical polishing liquid based on phytic acid-phytate according to claim 1, characterized in that: The particle size of the abrasive is 20nm-500nm.

6. A method for preparing a high-efficiency green chemical mechanical polishing liquid based on phytic acid-phytate according to any one of claims 1 to 5, characterized in that: The following steps are involved: Phytic acid, phytate, abrasive, H2O2 and deionized water are mixed to obtain the polishing liquid.

7. A polishing method using the efficient green chemical mechanical polishing liquid based on phytic acid-phytate as claimed in any one of claims 1 to 5, or the efficient green chemical mechanical polishing liquid based on phytic acid-phytate prepared by the preparation method according to claim 6, characterized in that: include: The polishing liquid is injected between the polishing pad and the TC4 titanium alloy at room temperature to perform chemical mechanical polishing on the TC4 titanium alloy. After the polishing is completed, the alloy is cleaned and dried to obtain the polished TC4 titanium alloy.

8. The polishing method according to claim 7, characterized in that: During the chemical mechanical polishing process, the rotation speed of the polishing pad is controlled to be 100 rpm to 500 rpm; The flow rate of the polishing liquid is 2mL / min to 5mL / min; The polishing pressure is 5MPa to 20MPa; The polishing time is 30min to 120min.

9. The polishing method according to claim 7, characterized in that: The polishing pad is made of polyurethane.

Citation Information

Cited By

  • Polishing solution for chemically mechanical polishing of silicon carbide wafer and preparation method of polishing solution

    CN122563485A