Perovskite-silicon-based laminated heterojunction solar cell, preparation method thereof and photovoltaic module

By forming an inorganic hole conductive layer and a [2-(9H-carbazol-9-yl)ethyl]phosphonic acid layer on a silicon heterojunction solar cell, combined with the co-evaporation technology of the perovskite layer, the problem on the surface of the silicon substrate is solved The problems of uneven coverage and low adhesion improve the stability and efficiency of perovskite-silicon-based stacked heterojunction solar cells.

CN118870933APending Publication Date: 2024-10-29TRINA SOLAR CO LTD +2
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410859957.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

When preparing high-efficiency tandem cells for existing commercial large textured silicon heterojunction solar cells, due to the irregular coverage of the silicon substrate surface and the low adhesion of the transparent conductive oxide layer, the perovskite and hole transport layers Uneven coverage reduces battery reliability and efficiency.

Method used

The radio frequency sputtering method is used to form an inorganic hole conductive layer on the conductive layer, and a [2-(9H-carbazol-9-yl)ethyl]phosphonic acid layer is spin-coated on the surface, combined with the co-evaporation technology of the perovskite layer. , forming a stable perovskite-silicon-based stacked heterojunction solar cell structure and improving the adhesion and interface consistency of the hole transport layer.

Benefits of technology

Through the use of inorganic hybrid hole transport layers, the stability and efficiency of the battery are improved, the convergence loss of interface electrons and holes is reduced, and the performance of the stacked battery is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118870933A_ABST
    Figure CN118870933A_ABST
Patent Text Reader

Abstract

The invention discloses a perovskite-silicon-based laminated heterojunction solar cell, a preparation method thereof and a photovoltaic module, and relates to the technical field of solar cells, and the method comprises the steps: forming a conductive layer on a silicon heterojunction solar cell; stacking a perovskite cell on the surface of the conductive layer to obtain a perovskite-silicon-based laminated heterojunction solar cell; wherein the perovskite cell comprises a hole transport layer; wherein the hole transport layer is prepared by forming a hole conductive layer on the surface of the conductive layer and forming a [2-(9H-carbazole-9-yl) ethyl] phosphonic acid layer on the surface of the hole conductive layer to obtain the hole transport layer, and the hole conductive layer is made of an inorganic hole transport material. According to the invention, the adhesive force between the hole transport layer and the surface of the heterojunction solar cell is improved, additional TCO parasitic absorption and shunting paths are avoided, balanced interface potential and matched energy level distribution are established, and the stability of the laminated cell is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular to a perovskite-silicon-based laminated heterojunction solar cell and a preparation method thereof, and a photovoltaic module. Background Art

[0002] In recent years, two-terminal stacked solar cell devices formed by superimposing new light-gain perovskites with traditional silicon-based materials have become a hot topic in low-cost, high-performance frontier research. However, how to directly use existing commercial large-textured silicon heterojunction cells to prepare high-efficiency stacked solar cell devices is an important problem that needs to be solved urgently.

[0003] Among them, the main challenge in preparing tandem cells is to integrate the two types of sub-cells through a series structure to form a conformal recombination junction (RJ). The core is to prepare the charge transport layer and the light gain perovskite layer on the silicon substrate after surface texturing. At present, most of the high-efficiency silicon-based tandem recombination junctions suitable for commercial manufacturing are used as electrodes in silicon heterojunction solar cells, which are composed of sputtered transparent conductive oxide (TCO) layers such as indium tin oxide (ITO), indium zinc oxide (IZO) and indium tungsten oxide (IWO). However, due to the irregular coverage of the pyramid surface of silicon heterojunction cells, it is very challenging to form conformal perovskites and hole transport layers (HTL) on the textured TCO. The main reason is the low adhesion between the organic HTL and the TCO, which reduces the reliability and service life of the cell.

[0004] Due to the low coverage of the hole transport layer on the transparent conductive oxide (TCO) surface, it is easy to cause a shunt path on the silicon surface in direct contact with the TCO of the perovskite top cell, resulting in a decrease in the short-circuit current of the cell and a decrease in the cell efficiency. Although the efficiency of the tandem crystalline silicon perovskite tandem cell can exceed 28% by effectively spin-coating self-assembled [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz) as a hole transport layer, it is unevenly and incompletely attached to the TCO surface, and the consistency of the perovskite material and the organic-inorganic interface layer is poor, resulting in low reliability.

[0005] It should be noted that the above content is not necessarily prior art, nor is it intended to limit the scope of patent protection of this application. Summary of the invention

[0006] The embodiments of the present application provide a perovskite-silicon-based stacked heterojunction solar cell and a preparation method thereof, and a photovoltaic module to solve one or more of the technical problems raised above.

[0007] A first aspect of an embodiment of the present application provides a method for preparing a perovskite-silicon-based stacked heterojunction solar cell, comprising:

[0008] forming a conductive layer on a silicon heterojunction solar cell;

[0009] A perovskite cell is stacked on the surface of the conductive layer to obtain a perovskite-silicon-based laminated heterojunction solar cell; wherein the perovskite cell includes a hole transport layer;

[0010] Among them, the preparation of the hole transport layer includes: forming a hole conductive layer on the surface of the conductive layer, forming a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer on the surface of the hole conductive layer to obtain a hole transport layer, and the material of the hole conductive layer is an inorganic hole transport material.

[0011] Optionally, forming a hole conductive layer on the surface of the conductive layer comprises:

[0012] At room temperature, the inorganic hole transport material is sputtered on the conductive layer by radio frequency sputtering to obtain the hole conductive layer.

[0013] Optionally, during the RF sputtering process, the chamber pressure is 0.3-0.5 Pa, the RF power is 100-120 W, the argon gas flow rate is 20-30 sccm, and the sputtering time is 5-10 minutes.

[0014] Optionally, the inorganic hole transport material is nickel oxide.

[0015] Optionally, forming a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer on the surface of the hole conductive layer comprises:

[0016] In a nitrogen atmosphere, an anhydrous ethanol solution containing [2-(9H-carbazole-9-yl)ethyl]phosphonic acid is spin-coated on the surface of the hole conductive layer, and then annealed to obtain a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer.

[0017] Optionally, the annealing temperature for the annealing treatment for forming the [2-(9H-carbazol-9-yl)ethyl]phosphonic acid layer is 100-120° C., and the annealing time is 5-25 minutes.

[0018] Optionally, the perovskite cell further includes a perovskite layer, and the preparation of the perovskite layer includes:

[0019] Co-evaporating PbI2 and CsBr to obtain a PbI2 / CsBr mixed layer;

[0020] Dissolving formamidine iodide, methylammonium bromide and methylammonium chloride in an ethanol solvent to obtain an organic salt solution;

[0021] The organic salt solution is spin-coated on the surface of the PbI2 / CsBr mixed layer and annealed to obtain the perovskite layer.

[0022] Optionally, the molar ratio of PbI2 and CsBr is (9-11):1;

[0023] The concentration of the formamidine iodine in the organic salt solution is 75-95 mg / mL, the concentration of the methylammonium bromide in the organic salt solution is 10-20 mg / mL, and the concentration of the methylammonium chloride in the organic salt solution is 5-15 mg / mL.

[0024] Optionally, the annealing temperature for the annealing treatment for preparing the perovskite layer is 150-200° C., and the annealing time is 15-20 minutes.

[0025] Optionally, the conductive layer is a transparent conductive oxide layer.

[0026] Optionally, the transparent conductive oxide layer is an indium tin oxide layer.

[0027] Optionally, forming a conductive layer on a silicon heterojunction solar cell comprises:

[0028] Deposition of indium tin oxide layer on silicon heterojunction solar cells using DC magnetron sputtering;

[0029] The pressure in the sputtering chamber is 8×10-5-10×10-5Pa, the pressure in the DC magnetron sputtering process is 0.35-0.5Pa, the O2 / Ar is adjusted to 1.0-1.5%, and the power density is 5.5-7kW / m 2 .

[0030] A second aspect of the embodiment of the present application provides a perovskite-silicon-based stacked heterojunction solar cell, comprising:

[0031] A silicon heterojunction cell having a first electrode;

[0032] A perovskite cell, comprising a hole transport layer, a perovskite layer, an electron transport layer, a first transparent conductive oxide layer and a second electrode stacked in sequence, wherein the hole transport layer comprises a hole conductive layer and a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer formed on the surface of the hole conductive layer, and the material of the hole conductive layer is an inorganic hole transport material;

[0033] A conductive layer located between the silicon heterojunction cell and the perovskite cell.

[0034] Optionally, the inorganic hole transport material is nickel oxide.

[0035] Optionally, the conductive layer is a second transparent conductive oxide layer.

[0036] Optionally, the second transparent conductive oxide layer is an indium tin oxide layer.

[0037] Optionally, the electron transport layer includes a LiF layer, a C60 layer, and a BCP layer stacked in sequence.

[0038] Optionally, an electron selective layer is further included between the first transparent conductive oxide layer and the electron transport layer.

[0039] Optionally, the material of the electron selective layer is tin dioxide.

[0040] Optionally, an anti-reflection layer is further disposed on the first transparent conductive oxide layer, and the second electrode is fixedly connected to the first transparent conductive oxide layer.

[0041] A third aspect of an embodiment of the present application provides a photovoltaic module, comprising at least one cell string, wherein the cell string comprises at least two perovskite crystalline silicon stacked cells as described above.

[0042] This application has the following beneficial effects:

[0043] (1) The present invention discloses a method for preparing a perovskite-silicon-based stacked heterojunction solar cell, which uses a metal oxide and a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer to prepare an inorganic hybrid hole transport layer, thereby improving the adhesion between the hole transport layer and the surface of the heterojunction solar cell, avoiding additional TCO parasitic absorption and shunting paths, establishing a balanced interface potential and matching energy level distribution, and improving the stability of the stacked cell.

[0044] (2) In the hole transport layer structure of the present application, due to the stronger chemical bonding force of organic matter, [2-(9H-carbazole-9-yl)ethyl]phosphonic acid can form a flat conformal layer with NiOx, and at the same time can passivate the corresponding surface defects, reduce the convergence loss of interface electrons and holes, and improve the battery efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.

[0046] Figure 1 It is a schematic structural diagram of the perovskite-silicon-based stacked heterojunction solar cell of the present application.

[0047] Figure 2 This is a flow chart for preparing perovskite-silicon-based stacked heterojunction solar cells in this application.

[0048] Figure 3 This is the flow chart of stacking perovskite cells in this application.

[0049] Explanation of the accompanying drawings: 1. Silicon heterojunction cell; 2. Perovskite cell; 3. Conductive layer; 10. First electrode; 20. Hole transport layer; 21. Perovskite layer; 22. Electron transport layer; 23. First transparent conductive oxide layer; 24. Second electrode; 25. Electron selection layer; 26. Anti-reflection layer. DETAILED DESCRIPTION

[0050] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, for clarity, the sizes of layers, regions, elements and their relative sizes may be exaggerated. Wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limitations on the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other.

[0051] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer or part discussed below can be represented as the second element, component, region, layer or part. And when the second element, component, region, layer or part is discussed, it does not mean that the present disclosure necessarily has the first element, component, region, layer or part.

[0052] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0053] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0054] To facilitate those skilled in the art to understand the technical solutions provided in the embodiments of the present application, the relevant technologies are described below:

[0055] like Figure 1 As shown, an embodiment of the present application provides a perovskite-silicon based stacked heterojunction solar cell, comprising: a silicon heterojunction cell 1, a perovskite cell 2, and a conductive layer 3 located between the silicon heterojunction cell 1 and the perovskite cell 2.

[0056] The silicon heterojunction battery 1 is provided with a first electrode 10 .

[0057] Specifically, the silicon heterojunction cell 1 can be a P-type silicon heterojunction cell or an N-type silicon heterojunction cell. In this embodiment, the silicon heterojunction cell 1 is preferably a P-type silicon heterojunction cell 1. In the P-type silicon heterojunction cell 1, an amorphous hydrogenated silicon layer prepared by plasma enhanced chemical vapor deposition (PECVD) is provided on the outer surface layer close to the P layer, and the preparation material is a composite junction of nc-SiOx-H(n) with a thickness of 5-10 nanometers.

[0058] The first electrode 10 is used as the back electrode of the perovskite-silicon based stacked heterojunction solar cell, and its material includes but is not limited to gold (Au), silver (Ag), aluminum (Al), and copper (Cu). In this embodiment, the first electrode 10 is an aluminum electrode.

[0059] Among them, the perovskite cell 2 includes a hole transport layer 20, a perovskite layer 21, an electron transport layer 22, a first transparent conductive oxide layer 23 and a second electrode 24 stacked in sequence, the hole transport layer 20 includes a hole conductive layer and a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz) layer formed on the surface of the hole conductive layer, and the material of the hole conductive layer is an inorganic hole transport material.

[0060] Specifically, the hole conductive layer in the hole transport layer 20 is located on the conductive layer 3 , and the [2-(9H-carbazol-9-yl)ethyl]phosphonic acid layer in the hole transport layer 20 is connected to the perovskite layer 21 .

[0061] The inorganic hole transport material includes but is not limited to nickel oxide (NiOx), titanium oxide (TiOx), and tin dioxide (SnO2). In this embodiment, the inorganic hole transport material is nickel oxide (NiOx).

[0062] In this embodiment, when nickel oxide (NiOx) is used as the hole conductive layer, its thickness is 20-30 nanometers, including any value within the thickness range, for example, 20 nanometers, 25 nanometers, and 30 nanometers.

[0063] The thickness of the [2-(9H-carbazol-9-yl)ethyl]phosphonic acid layer is 5-10 nanometers, including any value within the thickness range, for example, 5 nanometers, 8 nanometers, and 10 nanometers.

[0064] The preparation method of the hole transport layer will be described in detail below and will not be repeated in this embodiment.

[0065] The thickness of the perovskite layer 21 is 400-800 nanometers, including any value within the thickness range, for example, 400 nanometers, 500 nanometers, 600 nanometers, 700 nanometers, and 800 nanometers.

[0066] The main function of the electron transport layer 22 (ETL) is to transport electrons generated by the perovskite layer 21 and inhibit electron backflow. The electron transport layer 22 is usually composed of a material with good electronic conductivity and chemical stability. The materials of the electron transport layer 22 include one or more of tin dioxide (SnO2), titanium dioxide (TiO2), [6,6]-phenyl C61 butyric acid methyl ester (PC61BM), fullerene (C60), PDADI, LiF (lithium fluoride), and BCP (Bathocuproine, 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline).

[0067] The first transparent conductive oxide layer 23 is mainly used for charge transmission and conduction. The material of the first transparent conductive oxide layer 23 includes but is not limited to indium tin oxide (ITO), indium zinc oxide (IZO), aluminum zinc oxide (AZO), and indium antimony oxide (IAO).

[0068] The second electrode 24 is the front electrode of the perovskite-silicon-based laminated heterojunction solar cell, and is mainly used to send the generated current to the external circuit to form usable electric energy. The material of the second electrode 24 includes but is not limited to gold (Au), silver (Ag), aluminum (Al), and copper (Cu). In this embodiment, the second electrode 24 is an Ag electrode with a thickness of 100 nanometers.

[0069] The conductive layer 3 serves as a series structure layer between the silicon heterojunction cell 1 and the perovskite cell 2, which allows electrons to tunnel from one cell layer to another.

[0070] The conductive layer 3 is a second transparent conductive oxide layer. The material of the second transparent conductive oxide layer includes but is not limited to indium tin oxide (ITO), indium zinc oxide (IZO), aluminum zinc oxide (AZO), and indium antimony oxide (IAO). In this embodiment, when the second transparent conductive oxide layer is used as the conductive layer 3, it is preferably an indium tin oxide (ITO) layer.

[0071] This embodiment forms an inorganic hybrid hole transport layer 20 by combining a hole conductive layer prepared from an inorganic hole transport material and a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer, thereby avoiding the direct contact between the conductive layer 3 and the perovskite battery, resulting in a shunt path and parasitic absorption on the silicon surface, thereby establishing a balanced interface potential and a matching energy level distribution, and enhancing the stability of the stacked battery. In addition, the inorganic hybrid hole transport layer 20 in the present application is a conformal layer, which can also passivate the corresponding surface defects, reduce the convergence loss of interface electrons and holes, and thus improve the battery performance.

[0072] In an optional embodiment, in order to further improve the electron transport capability of the perovskite-silicon based stacked heterojunction solar cell, the electron transport layer 22 includes a LiF layer, a C60 layer, and a BCP layer stacked in sequence.

[0073] The thickness of the LiF layer is 1-2 nanometers, including any value within the thickness range, such as 1 nanometer, 1.5 nanometers, and 2 nanometers.

[0074] The thickness of the C60 layer is 20-30 nanometers, including any point value within this thickness range, for example, 20 nanometers, 25 nanometers, and 30 nanometers.

[0075] The thickness of the BCP layer is 3.5-6.5 nanometers, including any point value within this thickness range, for example, 3.5 nanometers, 5 nanometers, and 6.5 nanometers.

[0076] In an optional embodiment, in order to reduce the recombination of carriers and realize the effective collection of photogenerated carriers, an electron selective layer 25 is further included between the first transparent conductive oxide layer 23 and the electron transport layer 22 .

[0077] Specifically, the material of the electron selective layer 25 may be titanium oxide (TiO2), tin dioxide (SnO2), or the like.

[0078] In this embodiment, using a tin dioxide (SnO2) layer as an electron transport layer can form a low resistance to electrons and a high resistance to holes on the battery surface, thereby reducing surface recombination losses, and utilizing the excellent optical properties of SnO2 to broaden the absorption spectrum of the crystalline silicon battery.

[0079] In an optional embodiment, in order to reduce the reflection of light on the surface of the battery, thereby increasing the transmittance of light and improving the photoelectric conversion efficiency of the battery, an anti-reflection layer 26 is further provided on the first transparent conductive oxide layer 23, and the second electrode 24 is fixedly connected to the first transparent conductive oxide layer 23.

[0080] Specifically, the material of the anti-reflection layer 26 includes, but is not limited to, magnesium fluoride (MgFx), lithium fluoride (LiF), sodium fluoride (NaF), silicon oxide (SiO2), PDMS (polydimethylsiloxane), and silicon nitride (SiNx).

[0081] like Figure 2 As shown, the embodiment of the present application provides a method for preparing a perovskite-silicon-based stacked heterojunction solar cell, comprising the following steps:

[0082] S20, preparing a silicon heterojunction solar cell, and then forming a conductive layer on the silicon heterojunction solar cell;

[0083] The specific process is as follows:

[0084] A conductive layer is deposited on a silicon heterojunction solar cell by DC magnetron sputtering. In this embodiment, the conductive layer, wherein the pressure in the chamber of the sputtering device is 8×10-5-10×10-5Pa, the pressure during the DC magnetron sputtering process is 0.35-0.5Pa, O2 / Ar is adjusted to 1.0-1.5%, and the power density is 5.5-7kW / m 2 .

[0085] Specifically, the silicon heterojunction cell may be a P-type silicon heterojunction cell or an N-type silicon heterojunction cell. In this embodiment, the silicon heterojunction cell is a P-type silicon heterojunction cell.

[0086] The conductive layer is a transparent conductive oxide layer. The material of the transparent conductive oxide layer includes but is not limited to indium tin oxide (ITO), indium zinc oxide (IZO), aluminum zinc oxide (AZO), and indium antimony oxide (IAO). In this embodiment, when the transparent conductive oxide layer is used as the conductive layer, it is preferably an indium tin oxide (ITO) layer.

[0087] In this embodiment, the pressure in the chamber of the sputtering device is set to 8×10-5-10×10-5Pa, and the pressure is set to 0.35-0.5Pa during the DC magnetron sputtering process, the O2 / Ar is adjusted to 1.0-1.5%, and the power density is set to 5.5-7kW / m 2 , thereby improving the density of the conductive layer and further improving the film forming quality of the conductive layer.

[0088] S21, stacking perovskite cells on the surface of the conductive layer to obtain a perovskite-silicon-based stacked heterojunction solar cell.

[0089] See also Figure 3 , the stacked perovskite cell comprises:

[0090] S30, preparing a hole transport layer: forming a hole conductive layer on the surface of the conductive layer, forming a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer on the surface of the hole conductive layer to obtain a hole transport layer, wherein the material of the hole conductive layer is an inorganic hole transport material.

[0091] The specific process is as follows:

[0092] First, the surface of the conductive layer is cleaned, and after the cleaning is completed, an inorganic hole transport material is radio frequency sputtered on the conductive layer at room temperature to obtain a hole conductive layer.

[0093] In this embodiment, the inorganic hole transport material is nickel oxide (NiOx). During the RF sputtering process, the chamber pressure is 0.3-0.5 PaPa, the RF power is 100-120W, the argon flow rate is 20-30 sccm (Sputtering Rate per Square Centimeter), and the sputtering time is 5-10 minutes.

[0094] Secondly, after obtaining the hole conductive layer, a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer is formed on the surface of the hole conductive layer to obtain a hole transport layer. Specifically, an anhydrous ethanol solution in which [2-(9H-carbazole-9-yl)ethyl]phosphonic acid is dissolved is spin-coated on the surface of the hole conductive layer under a nitrogen atmosphere, and then annealed to obtain a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer.

[0095] In this example, the concentration of [2-(9H-carbazole-9-yl)ethyl]phosphonic acid in the anhydrous ethanol solution is 1.2 mg mL -1During spin coating, a solution of [2-(9H-carbazole-9-yl)ethyl]phosphonic acid in anhydrous ethanol was spin-coated on the surface of the nickel oxide (NiOx) layer at a speed of 3000 rpm in a nitrogen glove box for 30 seconds, and then annealed at a temperature of 100-120°C for 5-10 minutes.

[0096] In this embodiment, after spin coating the [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer on the surface of the nickel oxide (NiOx) layer, annealing is performed, and the annealing temperature is set to 100-120°C and the annealing time is set to 5-10 minutes, so that a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer with stronger bonding strength can be obtained, and the interface defects can be passivated.

[0097] S31. Prepare a perovskite layer.

[0098] The specific process is as follows: The perovskite layer is prepared by a two-step vapor phase thermal evaporation method.

[0099] First, PbI2 (lead iodide) and CsBr (cesium bromide) are co-evaporated to obtain a PbI2 / CsBr mixed layer. During the co-evaporation process, the molar ratio of PbI2 and CsBr is controlled to be (9-11):1, and the evaporation is stopped when the PbI2 / CsBr mixed layer with a total thickness of 350-400 nanometers is obtained.

[0100] Among them, other evaporation sources can also be used when performing co-evaporation, for example, using PbBr2 (lead bromide) and CsBr (cesium bromide), PbI2 (lead iodide) and CsI (cesium iodide), PbBr2 (lead bromide) and CsI (cesium iodide).

[0101] Secondly, formamidine iodine (FAI), methylammonium bromide (MABr), and methylammonium chloride (MACl) are dissolved in an ethanol solvent to obtain an organic salt solution, wherein the concentration of formamidine iodine in the organic salt solution is 75-95 mg / mL, the concentration of methylammonium bromide in the organic salt solution is 10-20 mg / mL, and the concentration of methylammonium chloride in the organic salt solution is 5-15 mg / mL.

[0102] The organic salt solution may also be prepared by dissolving at least other organic salts in an organic solvent.

[0103] The organic salt can be formamidine iodine (FAI), formamidine bromide (FABr), formamidine chloride (FACl), formamidine thiocyanate (FASCN), formamidine acetate (FACH3COO), methylamine iodine (MAI), methylammonium bromide (MABr), methylammonium chloride (MACl), methylamine acetate (MACH3COO), and methylamine thiocyanate (MASCN).

[0104] The organic solvent may be dimethylformamide (DMF), dimethyl sulfoxide (DMSO), ethanol (Ethanol), isopropyl ketone (IPA), ethyl acetate (Ethyl acetate), etc.

[0105] Finally, the PbI2 / CsBr blend layer was spin coated at 5000 rpm in air with RH (relative humidity) of 5% for 30 seconds to obtain a perovskite film layer, and then the perovskite film layer was annealed to obtain a perovskite layer, wherein the annealing temperature was 150-200°C and the annealing time was 15-20 minutes.

[0106] In this embodiment, after obtaining the perovskite film layer, the perovskite film layer is annealed, and the annealing temperature is set to 150-200°C, and the annealing time is set to 15-20 minutes, so as to improve the densification of the perovskite layer, so that the perovskite layer can better fit the suede surface of the silicon heterojunction battery.

[0107] S32, preparing an electron transport layer.

[0108] The specific process is as follows:

[0109] A LiF layer, a C60 layer, and a BCP layer are sequentially deposited on the perovskite layer by atomic layer deposition (ALD).

[0110] Among them, the thickness of the LiF layer is 1-2 nanometers, the thickness of the C60 layer is 20-30 nanometers, and the thickness of the BCP layer is 3.5-6.5 nanometers.

[0111] It should be noted that the material of the electron transport layer may also include one or more of tin dioxide (SnO2), titanium dioxide (TiO2), [6,6]-phenyl C61 butyric acid methyl ester (PC61BM), fullerene (C60), PDADI, LiF (lithium fluoride), and BCP (Bathocuproine, 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline).

[0112] The electron transport layer can also be prepared by thermal evaporation, solution coating, chemical vapor deposition (CVD), spin coating, etc.

[0113] In this embodiment, by using the LiF layer, the C60 layer, and the BCP layer as electron transport layers, a good energy level arrangement can be formed on the perovskite layer, which effectively improves the transmission and collection of electrons and hinders the transmission of holes on the interface.

[0114] S33, preparing a transparent conductive oxide layer;

[0115] Specifically, the preparation process of the transparent conductive oxide layer can refer to the preparation process of the conductive layer, and will not be described in detail in this embodiment.

[0116] S34. Prepare electrodes.

[0117] Specifically, the electrode can be prepared on the transparent conductive oxide layer by a thermal evaporation method, a screen printing method, or the like.

[0118] The material of the electrode includes but is not limited to gold (Au), silver (Ag), aluminum (Al), and copper (Cu).

[0119] The method for preparing a perovskite-silicon-based laminated heterojunction solar cell in this embodiment forms a hole conductive layer on the surface of the conductive layer when preparing the hole transport layer, and forms a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer on the surface of the hole conductive layer to obtain an inorganic hybrid hole transport layer, thereby avoiding the silicon surface shunt path and parasitic absorption caused by direct contact between the conductive layer and the perovskite cell, thereby establishing a balanced interface potential and matching energy level distribution, and enhancing the stability of the laminated cell. In addition, the inorganic hybrid hole transport layer in the present application is a conformal layer, which can also passivate the corresponding surface defects and reduce the convergence loss of interface electrons and holes, and the perovskite-silicon-based laminated heterojunction solar cell prepared by the above method has better cell performance.

[0120] The following will perform performance tests on the perovskite-silicon-based stacked heterojunction solar cells prepared by the preparation methods of the perovskite-silicon-based stacked heterojunction solar cells provided in the following embodiments and the perovskite-silicon-based stacked heterojunction solar cells of the relevant comparative examples, wherein the performance tests include the open circuit voltage Voc, short circuit current density Jsc, fill factor FF, and photoelectric conversion efficiency PCE of the battery device.

[0121] [Example 1]

[0122] The specific preparation process of a perovskite-silicon-based stacked heterojunction solar cell is as follows:

[0123] Step 1: prepare a silicon heterojunction solar cell, and then form a conductive layer on the silicon heterojunction solar cell, wherein the conductive layer is made of indium tin oxide (ITO) with a thickness of 50 nanometers.

[0124] Step 2: Prepare a hole transport layer in the perovskite cell on the conductive layer, wherein the hole transport layer includes a nickel oxide (NiOx) layer and a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer.

[0125] The specific preparation process is as follows:

[0126] First, a nickel oxide (NiOx) layer was RF sputtered on the conductive layer at room temperature. During the RF sputtering process, the chamber pressure was 0.39 Pa, the RF power was 100 W, the argon gas flow rate was 25 sccm, and the sputtering time was 8 min.

[0127] Secondly, an anhydrous ethanol solution containing [2-(9H-carbazole-9-yl)ethyl]phosphonic acid is spin-coated on the surface of the nickel oxide (NiOx) layer under a nitrogen atmosphere, and then annealed to obtain a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer. The concentration of [2-(9H-carbazole-9-yl)ethyl]phosphonic acid in the anhydrous ethanol solution is 1.5 mg mL-1, the spin-coating speed is 3000 rpm, the spin-coating time is 30 seconds, the annealing temperature is 120°C, and the annealing time is 15 minutes.

[0128] Step 3: Prepare a perovskite layer on the hole transport layer by a two-step vapor phase thermal evaporation method, wherein the thickness of the perovskite layer is 600 nanometers.

[0129] Step 4: preparing an electron transport layer on the perovskite layer, wherein the electron transport layer includes a LiF layer with a thickness of 1.5 nanometers, a C60 layer with a thickness of 25 nanometers, and a BCP layer with a thickness of 5 nanometers, which are stacked in sequence.

[0130] Step 5: Prepare a transparent conductive oxide layer on the electron transport layer, wherein the material of the transparent conductive oxide layer is indium tin oxide (ITO) with a thickness of 50 nanometers.

[0131] Step 6: Prepare an electrode on the transparent conductive oxide layer.

[0132] [Example 2]

[0133] The perovskite crystalline silicon stacked cell of Example 2 was prepared by referring to the preparation method of Example 1, except that the sputtering time in step 2 of Example 2 when preparing the nickel oxide (NiOx) layer was 20 minutes.

[0134] [Example 3]

[0135] The perovskite crystalline silicon stacked cell of Example 3 was prepared by referring to the preparation method of Example 1, except that the sputtering time in preparing the nickel oxide (NiOx) layer in step 2 of Example 3 was 25 minutes.

[0136] [Example 4]

[0137] The perovskite crystalline silicon stacked cell of Example 4 was prepared by referring to the preparation method of Example 1, the only difference being that the nickel oxide (NiOx) layer prepared in step 2 of Example 4 was replaced by a titanium oxide (TiOx) layer, and the other preparation processes were the same.

[0138] [Example 5]

[0139] The perovskite crystalline silicon stacked cell of Example 5 is prepared by referring to the preparation method of Example 2, the only difference being that the nickel oxide (NiOx) layer prepared in step 2 of Example 5 is replaced by a titanium oxide (TiOx) layer, and the other preparation processes are the same.

[0140] [Example 6]

[0141] The perovskite crystalline silicon stacked cell of Example 6 is prepared by referring to the preparation method of Example 3, the only difference being that the nickel oxide (NiOx) layer prepared in step 2 of Example 6 is replaced by a titanium oxide (TiOx) layer, and the other preparation processes are the same.

[0142] [Comparative Example 1]

[0143] The perovskite crystalline silicon stacked cell of Example 7 was prepared by referring to the preparation method of Example 1, except that the hole transport layer prepared in step 2 only includes a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer.

[0144] The test data is shown in the following table:

[0145]

[0146]

[0147] It can be seen from Table 1 above that the perovskite-silicon-based stacked heterojunction solar cells prepared by the methods in Examples 1 to 6 have better performance and stability than the perovskite-silicon-based stacked heterojunction solar cells prepared by the method in Comparative Example 1.

[0148] The embodiment of the present application may also provide a photovoltaic module (not shown), including at least one battery string, the battery string includes at least two perovskite-silicon-based stacked heterojunction solar cells as described above, and adjacent solar cells can be connected together by series welding.

[0149] It should be noted that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The orientation words "inside" and "outside" refer to the inside and outside relative to the outline of each component itself. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Therefore, the exemplary term "above..." can include both "above..." and "below..." orientations. The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here are interpreted accordingly.

[0150] It should also be noted that "one embodiment", "another embodiment", "embodiment", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Further, when a specific feature, structure or characteristic is described in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.

[0151] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0152] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A method for preparing a perovskite-silicon-based stacked heterojunction solar cell, It is characterized in that The following steps are involved: forming a conductive layer on a silicon heterojunction solar cell; A perovskite cell is stacked on the surface of the conductive layer to obtain a perovskite-silicon-based laminated heterojunction solar cell; wherein the perovskite cell includes a hole transport layer; Among them, the preparation of the hole transport layer includes: forming a hole conductive layer on the surface of the conductive layer, forming a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer on the surface of the hole conductive layer to obtain a hole transport layer, and the material of the hole conductive layer is an inorganic hole transport material.

2. The method for preparing a perovskite-silicon-based laminated heterojunction solar cell according to claim 1, It is characterized in that Forming a hole conductive layer on the surface of the conductive layer comprises: At room temperature, the inorganic hole transport material is sputtered on the conductive layer by radio frequency sputtering to obtain the hole conductive layer.

3. The method for preparing a perovskite-silicon-based laminated heterojunction solar cell according to claim 2, It is characterized in that During the RF sputtering process, the chamber pressure is 0.3-0.5 Pa, the RF power is 100-120 W, the argon flow rate is 20-30 sccm, and the sputtering time is 5-10 minutes.

4. The method for preparing a perovskite-silicon-based laminated heterojunction solar cell according to claim 1, It is characterized in that The inorganic hole transport material is nickel oxide.

5. The method for preparing a perovskite-silicon-based laminated heterojunction solar cell according to claim 1, It is characterized in that Forming a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer on the surface of the hole conductive layer comprises: In a nitrogen atmosphere, an anhydrous ethanol solution containing [2-(9H-carbazole-9-yl)ethyl]phosphonic acid is spin-coated on the surface of the hole conductive layer, and then annealed to obtain a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer.

6. The method for preparing a perovskite-silicon-based stacked heterojunction solar cell according to claim 5, It is characterized in that The annealing temperature for the annealing treatment for forming the [2-(9H-carbazol-9-yl)ethyl]phosphonic acid layer is 100-120° C., and the annealing time is 5-25 minutes.

7. The method for preparing a perovskite-silicon-based stacked heterojunction solar cell according to any one of claims 1 to 6, It is characterized in that The perovskite cell further comprises a perovskite layer, and the preparation of the perovskite layer comprises: PbI 2 Co-evaporation with CsBr yields PbI 2 / CsBr blended layer; Dissolving formamidine iodide, methylammonium bromide and methylammonium chloride in an ethanol solvent to obtain an organic salt solution; The organic salt solution was spin-coated on PbI 2 On the surface of the CsBr / CsBr mixed layer, annealing treatment is performed to obtain the perovskite layer.

8. The method for preparing a perovskite-silicon-based stacked heterojunction solar cell according to claim 7, It is characterized in that The PbI 2 The molar ratio of CsBr is (9-11):1; The concentration of the formamidine iodine in the organic salt solution is 75-95 mg / mL, the concentration of the methylammonium bromide in the organic salt solution is 10-20 mg / mL, and the concentration of the methylammonium chloride in the organic salt solution is 5-15 mg / mL.

9. The method for preparing a perovskite-silicon-based laminated heterojunction solar cell according to claim 7, It is characterized in that The annealing temperature for the annealing treatment of preparing the perovskite layer is 150-200° C., and the annealing time is 15-20 minutes.

10. The method for preparing a perovskite-silicon-based stacked heterojunction solar cell according to claim 1, It is characterized in that The conductive layer is a transparent conductive oxide layer.

11. The method for preparing a perovskite-silicon-based stacked heterojunction solar cell according to claim 10, It is characterized in that The transparent conductive oxide layer is an indium tin oxide layer.

12. The method for preparing a perovskite-silicon-based tandem heterojunction solar cell according to claim 11, It is characterized in that The step of forming a conductive layer on a silicon heterojunction solar cell comprises: Deposition of indium tin oxide layer on silicon heterojunction solar cells using DC magnetron sputtering; The pressure inside the sputtering chamber is 8×10 -5 -10×10 -5 Pa, the pressure in the DC magnetron sputtering process is 0.35-0.5Pa, O 2 / Ar is adjusted to 1.0-1.5%, and the power density is 5.5-7kW / m 2 .

13. A perovskite-silicon based stacked heterojunction solar cell, It is characterized in that include: A silicon heterojunction cell having a first electrode; A perovskite cell, comprising a hole transport layer, a perovskite layer, an electron transport layer, a first transparent conductive oxide layer and a second electrode stacked in sequence, wherein the hole transport layer comprises a hole conductive layer and a [2-(9H-carbazole-9-yl)ethyl]phosphonic acid layer formed on the surface of the hole conductive layer, and the material of the hole conductive layer is an inorganic hole transport material; A conductive layer located between the silicon heterojunction cell and the perovskite cell.

14. The perovskite-silicon based tandem heterojunction solar cell according to claim 13, It is characterized in that The inorganic hole transport material is nickel oxide.

15. The perovskite-silicon based tandem heterojunction solar cell according to claim 13, It is characterized in that The conductive layer is a second transparent conductive oxide layer.

16. The perovskite-silicon based tandem heterojunction solar cell according to claim 15, It is characterized in that The second transparent conductive oxide layer is an indium tin oxide layer.

17. The perovskite-silicon based tandem heterojunction solar cell according to any one of claims 13 to 16, It is characterized in that The electron transport layer includes a LiF layer, a C60 layer, and a BCP layer stacked in sequence.

18. The perovskite-silicon based tandem heterojunction solar cell according to claim 13, It is characterized in that An electron selection layer is further included between the first transparent conductive oxide layer and the electron transport layer.

19. The perovskite-silicon based tandem heterojunction solar cell according to claim 13, It is characterized in that The material of the electron selective layer is tin dioxide.

20. The perovskite-silicon based tandem heterojunction solar cell according to claim 13, It is characterized in that An anti-reflection layer is also disposed on the first transparent conductive oxide layer, and the second electrode is fixedly connected to the first transparent conductive oxide layer.

21. A photovoltaic module, It is characterized in that include: At least one cell string, the cell string comprising at least two perovskite-silicon-based tandem heterojunction solar cells according to any one of claims 13 to 20.

Citation Information

Cited By

  • Perovskite solar cell module self-assembled monomolecular hole transport material and preparation method thereof

    CN119504856A

  • Photovoltaic cell with two laminated ends

    CN121240678A