Self-supporting alloy catalytic electrode with three-dimensional porous structure and preparation method of self-supporting alloy catalytic electrode
By changing the solvent composition of the electrodeposited liquid, an alloy catalytic electrode with a three-dimensional porous structure is solved, and the catalytic electrode activity of nickel mesh in the prior art is improved, and the efficiency and cost-effectiveness of alkaline electrolysis hydrogen production is improved. It is suitable for industrial applications. .
Patent Information
- Application Number
- CN202411138772.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-01
AI Technical Summary
Among the existing alkaline electrolytic hydrogen production technology, the intrinsic catalytic activity of commercial nickel mesh catalytic electrodes is poor, resulting in low working current density and high power consumption, increasing the cost of hydrogen production and making it difficult to meet the needs of large-scale applications.
By changing the solvent composition of the electrodeposition solution, an organic alcohol solution is introduced to regulate the size and number of bubbles during the electrodeposition process, forming a self-supported alloy catalytic electrode rich in three-dimensional porous structures to improve the density and stability of the active site.
It significantly improves catalytic activity, reduces the cost of hydrogen production of alkaline electrolytic water, improves the working efficiency of the electrolytic cell, and is suitable for large-scale industrial production.
Smart Images

Figure HDA0005000149560000011 
Figure HDA0005000149560000012 
Figure HDA0005000149560000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrocatalysis, and in particular relates to a self-supporting alloy catalytic electrode with a three-dimensional porous structure and a preparation method thereof. Background Art
[0002] Hydrogen energy is a green and efficient secondary energy source, and it occupies a very important position in the diversified clean energy system. At present, there are mainly the following ways to produce hydrogen in industry: hydrogen production from fossil energy reforming, hydrogen production from industrial by-product gas, and hydrogen production from water electrolysis. Compared with the first two technical routes, hydrogen production from water electrolysis has great advantages in energy conservation, emission reduction and sustainable development, and is the main body of hydrogen supply in the future. Among them, alkaline water electrolysis has the advantages of simple equipment, high purity of hydrogen production and low cost, and has received widespread attention. At present, commercial alkaline electrolyzers mainly choose nickel mesh as the catalytic electrode, and apply a certain cell pressure under high concentration KOH solution and 80°C working conditions to electrolyze water to produce hydrogen. Although the widely used commercial nickel mesh has good stability at industrial-grade current density, its intrinsic catalytic activity is poor, resulting in low working current density (<3000Am 2 ) and high power consumption (>4.5KWh Nm 3 ), which greatly increases the cost of hydrogen production by alkaline water electrolysis. Therefore, it is urgent to prepare catalytic electrodes with high catalytic activity, high active site density and high stability to promote the large-scale application of hydrogen production by alkaline water electrolysis.
[0003] In recent years, researchers have found that a porous metal deposition layer can be constructed on a planar conductive substrate by electrodeposition, which can increase the specific surface area of the catalytic electrode, expose more active sites, and optimize the intrinsic hydrogen evolution activity of the electrode. At the same time, the high interfacial bonding force brought by the electrodeposition method also ensures the high structural stability of the electrode. For example, patent application CN202110435341.1 discloses a porous nickel mesh electrolysis catalyst and a preparation method thereof. A nickel metal particle layer is loaded on the surface of a commercial nickel mesh by electrodeposition. Since the hydrogen generated by the cathode during the deposition process is adsorbed on the electrode surface, the metal deposition layer grows along the edge of the bubble, thereby forming a porous nickel metal deposition structure. Patent application CN 202410059680.8 discloses a highly active nickel-based electrocatalyst for alkaline water electrolysis and a preparation method thereof. The method constructs a multi-metal deposition layer of two or more metal combinations on the surface of a commercial nickel mesh by electrodeposition by changing the solute composition of the metal salt in the electrodeposition solution. The resulting electrode has good catalytic activity. However, the above scheme uses ordinary electrodeposition to obtain a dense metal particle deposition layer with large and single surface pores and a limited number of exposed active sites, which still cannot meet the actual production application needs. Therefore, it is of great research significance and practical value to make reasonable improvements based on the existing electrodeposition technology, optimize the size of the deposited metal particles and the porous structure of the deposition layer, and construct an alkaline hydrogen evolution electrode with high-density active sites and high stability in one step. Summary of the invention
[0004] The main purpose of the present invention is to provide a self-supporting alloy catalytic electrode rich in three-dimensional porous structure in view of the problems and shortcomings of the prior art, which has a smaller alloy particle size and a three-dimensional pore structure with a larger exposed area, and can show significantly enhanced hydrogen evolution activity.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for preparing a self-supporting alloy catalytic electrode with a three-dimensional porous structure comprises the following steps:
[0007] 1) preparing an electrodeposition solution: dissolving two metal salts (different metal salts) uniformly in water and an organic alcohol solution respectively to obtain a salt alcohol solution and a salt water solution respectively; then adding the obtained salt water solution to the salt alcohol solution, stirring uniformly, to obtain a uniform and stable electrodeposition solution;
[0008] 2) A two-electrode system is used, with a conductive substrate as the cathode, the cathode and the anode are immersed in an electrodeposition solution, electrochemical deposition is performed, and then washed and dried to obtain a self-supporting alloy catalytic electrode with a three-dimensional porous structure.
[0009] In the above scheme, the selected planar conductive substrate is one of nickel mesh, nickel sheet, nickel foam, titanium mesh, titanium sheet, carbon cloth, carbon paper, copper foam, graphene film, etc.
[0010] In the above scheme, in step 1), the saline solution is slowly added to the saline alcohol solution at a flow rate of 10-20 mL / min.
[0011] In the above scheme, the concentration of the metal salt (one of the two metal salts) in the organic salt alcohol solution is 0.5-2.5 mol / L.
[0012] In the above scheme, the concentration of the metal salt (the other of the two metal salts) in the saline solution is 0.01-0.05 mol / L.
[0013] Furthermore, the volume ratio of the saline-alcohol solution to the saline solution is 1-10:1.
[0014] Furthermore, the organic alcohol can be selected from one or more of methanol, ethanol, isopropanol, ethylene glycol, glycerol, etc. Furthermore, the electrodeposition solution also introduces one of ammonium chloride, ammonium fluoride, sodium citrate, boric acid, etc. as an electrodeposition auxiliary agent; the amount of the auxiliary agent introduced is 1-2 mol / L.
[0015] In the above scheme, the two metal salts in step 1) are specifically selected from two of nickel salts, iron salts, cobalt salts, manganese salts, zirconium salts, titanium salts, copper salts, cerium salts, tungstates, vanadates, molybdates, etc.
[0016] Furthermore, the conductive substrate is pretreated before use, and the pretreatment step includes: cutting the conductive substrate, ultrasonically cleaning it with acetone, ethanol, hydrochloric acid and water in sequence, and then drying it naturally.
[0017] In the above scheme, in the electrochemical deposition step, the applied current density is 0.1-3A / cm 2 , the deposition time is 90-600s.
[0018] The self-supporting alloy catalytic electrode prepared according to the above scheme has a large number of macropores with a diameter of 8-50μm distributed on the surface of the alloy particle (metal particle size is 0.5-5μm) deposition layer, and a large number of particle accumulation pores with a diameter of 0.5-5μm are evenly distributed on the surface and inside of the alloy particle deposition layer, which together form a hierarchical pore structure, which can more effectively expose high-efficiency active sites; at the same time, the strong bonding force between the catalytic layer and the substrate ensures the mechanical strength and chemical stability of the obtained electrode, so that the obtained electrode has a longer service life.
[0019] The reaction principle of the present invention is:
[0020] On the basis of constructing a porous metal nanoparticle deposition layer by conventional electrodeposition, the solvent composition of the deposition liquid is changed, and a certain proportion of organic alcohol solution is introduced into the aqueous deposition liquid. The viscosity of the deposition liquid is changed by taking advantage of the different surface tensions of the organic alcohol solution and the aqueous solution, thereby changing the size and number of hydrogen bubbles generated by electrolysis during the deposition process, changing the pore structure in the metal particle deposition layer and the size of the deposited metal particles, and finally obtaining a self-supporting electrode material uniformly loaded with a metal particle deposition layer rich in a three-dimensional hierarchical porous structure.
[0021] It should be emphasized that the ratio of water to organic alcohol solution in the electrodeposition solution must be controlled within a certain range. If it is below this range, a rich pore structure cannot be constructed, and if it is above this range, the metal deposition particles will fall off.
[0022] In addition, when preparing the electrodeposition solution, the present invention needs to proceed in the order of slowly adding the salt solution to the salt alcohol solution, utilizing the poor solubility of metal salts in alcohol solutions to leave insoluble metal salt particles. During the electrodeposition process, the insoluble particles will be adsorbed onto the surface of the substrate as nucleation seeds, which is beneficial to promoting the uniform formation of the porous structure and effectively enhancing the bonding force between the deposited layer and the substrate.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) Compared with the traditional electrodeposition method, the present invention adjusts the size and number of bubbles generated during the electrodeposition process by adjusting the viscosity of the electrodeposition liquid, and uses the generated bubbles as a template to uniformly deposit a nano-metal particle layer rich in a three-dimensional porous structure on a planar conductive substrate. The nano-metal particle layer has a richer porous structure, can effectively expose more metal active sites, and improve the unit active site density.
[0025] (2) Taking advantage of the poor solubility of metal salts in alcohol solutions, insoluble nanoparticles are introduced into the electrodeposition solution; during the electrodeposition process, they can be directly adsorbed on the surface of the conductive substrate as electrodeposition nucleus seeds, which can effectively reduce the interface formation energy, skip the basic nucleation process, and is beneficial to the structure formation and uniform growth of the porous alloy catalyst layer.
[0026] (3) Compared with the currently widely used commercial nickel mesh, Raney nickel, and porous nickel-based electrodes obtained by traditional electrodeposition, the self-supporting three-dimensional porous alloy catalytic electrode prepared in the present invention has higher catalytic activity, can effectively improve the working efficiency of the electrolyzer, and significantly reduce the cost of hydrogen production by alkaline water electrolysis.
[0027] (4) The preparation cycle involved in the present invention is short, the operation is simple, the repeatability is strong, and it is suitable for large-scale industrial production. It has good application prospects in the field of water electrolysis and hydrogen production. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic diagram of the preparation process of Example 1 of the present invention;
[0029] Figure 2 This is a scanning electron microscope image of the final product prepared in Example 1 of the present invention;
[0030] Figure 3 The electrochemical polarization curve of the final product prepared in Example 1 of the present invention is shown;
[0031] Figure 4 This is a scanning electron microscope image of the final product prepared in Comparative Example 1 of the present invention;
[0032] Figure 5 This is a scanning electron microscope image of the final product prepared in Comparative Example 2 of the present invention;
[0033] Figure 6 This is a scanning electron microscope image of the final product prepared in Comparative Example 3 of the present invention.
[0034] Figure 7 This is a scanning electron microscope image of the final product prepared in Example 2 of the present invention;
[0035] Figure 8 This is a scanning electron microscope image of the final product prepared in Example 3 of the present invention;
[0036] Fig. 9 This is the electrochemical polarization curve diagram of the final product prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0038] Example 1
[0039] A self-supporting alloy catalytic electrode with a three-dimensional porous structure, the synthesis process diagram is shown in Figure 1 , the specific preparation method comprises the following steps:
[0040] 1) Pretreatment of conductive substrate material: A 46-mesh skew-woven commercial nickel mesh was selected as the electrodeposition substrate material, which was cut into a standard size (2*2 cm) and then ultrasonically cleaned with acetone, ethanol, 3M hydrochloric acid, and deionized water in sequence, and then naturally dried for standby use;
[0041] 2) preparing an electrodeposition solution: uniformly dispersing 0.002 mol of ferrous sulfate and 0.2 mol of nickel chloride in 100 mL of deionized water and 400 mL of ethylene glycol, respectively, then adding the saline solution to the saline alcohol solution at a rate of 10 mL / min, and adding 2 M ammonium chloride, slowly stirring to obtain an electrodeposition solution for standby use;
[0042] 3) The nickel mesh treated in step 1) is used as the cathode, the graphite sheet is used as the anode, the positive and negative electrodes of a DC power supply are connected to the graphite sheet and the pretreated nickel mesh respectively, and the electrodes are immersed in the electrodeposition solution; at room temperature, the deposition current is set to 0.5 A cm -2 After the electrodeposition is completed, the electrode is rinsed with deionized water and dried naturally to obtain a self-supporting three-dimensional porous nickel-iron / nickel (3D porous NiFe / Ni) electrode.
[0043] Figure 2 The scanning electron microscope images of the self-supporting NiFe electrode and the 3D porous NiFe / Ni electrode obtained by electroplating a commercial nickel mesh, a deposition solution prepared with pure water as the solvent. It can be seen from the figure that the commercial nickel mesh is woven from nickel metal wire, and its surface is smooth and has an extremely low specific surface area, resulting in insufficient exposure of active sites. When nickel salt and iron salt are dissolved in pure water to prepare a deposition solution, and a nickel-iron alloy deposition layer is constructed on the surface of the commercial nickel mesh by electrodeposition, the surface roughness of the nickel mesh is significantly improved. At this time, the particle size of the metal particles obtained is about 3-5μm. At the same time, due to the adsorption of hydrogen generated by the cathode on the surface of the nickel mesh during the electrolysis process, this serves as a template for the nickel metal particle deposition layer to have a certain pore structure (pore size is about 10-15μm), which increases the effective active area of the electrode. At the same deposition current and deposition time (0.5A cm -2 / 540s), the self-supporting electrode obtained by the electrodeposition scheme involved in the present invention shows a more obvious hierarchical porous structure (large pores with a diameter of 20-50μm, and particle accumulation pores with a diameter of about 3-5μm distributed on the surface and inside of the deposition layer), the particle size of the metal particles in the deposition layer is further reduced (the particle size is about 1-2μm), its surface is rougher, the metal nickel particle size and the pore structure of the deposition layer are richer, and it has a significantly increased effective active area, which is conducive to the rapid transmission and diffusion of reactants and gas products.
[0044] Figure 3The electrochemical polarization curves of commercial nickel mesh, self-supporting NiFe electrode obtained by electrodeposition using a deposition solution prepared with pure water, and 3Dporous NiFe / Ni electrode at room temperature with 1M KOH are shown in the figure. It can be seen from the figure that loading a porous metal deposition layer on the surface of the nickel mesh can effectively improve the hydrogen evolution activity of the nickel mesh electrode, and the nickel mesh electrode deposited with three-dimensional porous nickel-iron metal particles after optimizing the electrodeposition strategy of the present invention shows a lower hydrogen evolution overpotential. Under the conditions of 1M KOH and room temperature, the driving current of 1A cm -2 The hydrogen evolution current only requires 540mV overpotential, which is 150mV lower than that of conventional electrodeposited nickel-iron electrodes. The results show that the self-supporting electrode prepared by our method has stronger hydrogen evolution activity under industrial-grade alkaline hydrogen evolution conditions. This excellent performance is of great significance for practical industrial applications.
[0045] Comparative Example 1
[0046] An alloy catalytic electrode, the preparation method of which comprises the following steps:
[0047] 1) Pretreatment of conductive substrate material: A 46-mesh skew-woven commercial nickel mesh was selected as the electrodeposition substrate material, which was cut into a standard size (2*2 cm) and then ultrasonically cleaned with acetone, ethanol, 3M hydrochloric acid, and deionized water in sequence, and then naturally dried for standby use;
[0048] 2) preparing an electrodeposition solution: 0.002 mol of ferrous sulfate and 1 mol of nickel chloride were uniformly dispersed in 100 mL of deionized water and 1500 mL of ethylene glycol, respectively, and then the saline solution was added to the salt alcohol solution at a rate of 15 mL / min, and 2 M ammonium chloride was added, and the electrodeposition solution was slowly stirred for standby use;
[0049] 3) The nickel mesh treated in step 1) is used as the cathode, the graphite sheet is used as the anode, the positive and negative electrodes of a DC power supply are connected to the graphite sheet and the pretreated nickel mesh respectively, and the electrodes are immersed in the electrodeposition solution; at room temperature, the deposition current is set to 0.5 A cm -2 , and the electrodeposition treatment was carried out for 540 seconds. After the deposition, the obtained electrode was rinsed with deionized water and dried naturally to obtain an electrode.
[0050] Figure 4 This is a scanning electron microscope image of the electrode obtained in Comparative Example 1. As can be seen from the figure, when the proportion of organic alcohol (ethylene glycol) is too high, gas will be generated violently during the electrolysis process, and the bonding force between the metal particle deposition layer and the nickel mesh substrate will be seriously affected, resulting in the fall-off of nickel metal particles and difficulty in forming a deposition layer.
[0051] Comparative Example 2
[0052] An alloy catalytic electrode, the preparation method of which is substantially the same as that of comparative example 1, except that the mass ratio of water to ethylene glycol introduced in step 2) is 30:1.
[0053] Figure 5 This is a scanning electron microscope image of the electrode obtained in Comparative Example 2. It can be seen from the figure that when the proportion of organic alcohol is too low, a good three-dimensional hierarchical porous structure cannot be formed.
[0054] Comparative Example 3
[0055] An alloy catalytic electrode, whose preparation method is roughly the same as that of comparative example 1, except that: 100 mL of pure water is directly mixed with 400 mL of ethylene glycol, and then 0.2 mol of nickel chloride, 0.002 mol of ferrous sulfate and 2M ammonium chloride are added thereto at the same time, stirred evenly and used directly as an electrodeposition solution.
[0056] Figure 6 This is a scanning electron microscope image of the electrode obtained in Comparative Example 3. As can be seen from the figure, the size difference between the alloy particles in the electrodeposited layer obtained in this embodiment is too large (3-20 μm), and a large number of particles are agglomerated, resulting in a loose structure and uneven distribution of the deposition layer, which affects the final electrocatalytic hydrogen evolution performance.
[0057] Example 2
[0058] A self-supporting three-dimensional porous cobalt-molybdenum-nickel catalytic electrode with a three-dimensional porous structure, the preparation method of which comprises the following steps:
[0059] 1) Pretreatment of conductive substrate material: A 46-mesh skew-woven commercial nickel mesh was selected as the electrodeposition substrate material, which was cut into a standard size (2*2 cm) and then ultrasonically cleaned with acetone, ethanol, 3M hydrochloric acid, and deionized water in sequence, and then naturally dried for standby use;
[0060] 2) preparing an electrodeposition solution: 0.01 mol of cobalt chloride and 0.4 mol of ammonium molybdate are uniformly dispersed in 500 mL of deionized water and 750 mL of ethylene glycol, respectively, and then the saline solution is added to the saline alcohol solution at a flow rate of 15 mL / min, and 1 M sodium citrate is added, and the electrodeposition solution is slowly stirred for standby use;
[0061] 3) Using the nickel mesh treated in step 1) as the cathode and the graphite sheet as the anode, the positive and negative electrodes of a DC power supply are connected to the graphite sheet and the pretreated nickel mesh respectively, and the electrodes are immersed in the electrodeposition solution; at room temperature, the current density is maintained at 3A cm -2 , and the electrodeposition treatment was carried out for 60s, 90s, and 120s, respectively, and self-supporting three-dimensional porous cobalt-molybdenum / nickel (3D porous CoMo / Ni) electrodes were obtained.
[0062] Figure 7 This is a scanning electron microscope image of the electrode obtained by the scheme described in Example 2. It can be seen from the figure that the surface of the obtained electrode is evenly covered with a porous deposition layer formed by alloy particles with a particle size of about 1-3μm. On the surface of the cobalt-molybdenum alloy deposition layer, a large number of macropores with an average diameter of 15μm are evenly distributed, and at the same time, small pore structures with a pore size range of 500nm-5μm are also distributed in the alloy particle deposition layer. The successful construction of the porous cobalt-molybdenum alloy deposition layer obtained in this example and the porous nickel metal deposition layer in Example 1 proves that the scheme for constructing graded porous alloy electrodes proposed in the present invention is universal in terms of metal element selection.
[0063] Example 3
[0064] A self-supporting three-dimensional porous cobalt-nickel / nickel catalytic electrode with a three-dimensional porous structure, the preparation method of which comprises the following steps:
[0065] 1) Pretreatment of conductive substrate material: Use a 46-mesh oblique woven commercial nickel mesh as the electrodeposition substrate material, cut it into a standard size (2*2 cm), and ultrasonically clean it with acetone, ethanol, 3M hydrochloric acid, and deionized water in sequence, and then dry it naturally for use;
[0066] 2) preparing the electrodeposition solution: on the premise of ensuring that the total amount of the metal salt solute is 1M, nickel chloride and cobalt chloride are taken in a certain ratio (Ni and Co molar ratios are 1:1, 4:1 and 6:1, respectively), dispersed in 400mL of pure water and 1000mL of ethanol, respectively, and then the salt solution is added to the salt alcohol solution at a flow rate of 10mL / min, and 2M ammonium chloride is added as an electrodeposition auxiliary agent, and slowly stirred to obtain the electrodeposition solution for standby use;
[0067] 3) Using the nickel mesh treated in step 1) as the cathode and the graphite sheet as the anode, connecting the positive and negative electrodes of a DC power supply to the graphite sheet and the pretreated nickel mesh respectively, and immersing the electrodes in an electrodeposition solution; maintaining a current density of 0.5 A cm at room temperature; -2 , and an electrodeposition treatment was performed for 120 s to obtain a self-supporting three-dimensional porous cobalt nickel / nickel (3D porousCoNi / Ni) electrode.
[0068] Figure 8 This is a scanning electron microscope image of the electrode obtained in Example 3. It can be seen from the figure that the surface of the obtained electrode is evenly covered with a porous deposition layer formed by alloy particles with a particle size of about 1-3μm. A large number of macropores with an average diameter of 10-20μm are evenly distributed on the surface of the cobalt-nickel alloy deposition layer. At the same time, a particle accumulation pore structure with a pore size range of 3-5μm is also distributed in the deposition layer. Fig. 9 This is the electrochemical polarization curve of the electrode obtained in Example 3.
[0069] It can be seen that the three-dimensional porous structure can be constructed by the above scheme of the present invention, which significantly enhances the electrocatalytic hydrogen evolution activity; compared with the NiCo self-supporting electrode obtained by directly mixing the composite metal salt with the alcohol aqueous solution and then electrodepositing it, the Ni:Co=1:1 three-dimensional porous self-supporting electrode constructed in this embodiment drives 1A cm -2 The overpotential required for the hydrogen evolution current density is only 480 mV, which is reduced by 220 mV.
[0070] The above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, so the obvious changes or modifications derived are still within the protection scope of the invention.
Claims
1. A method for preparing a self-supporting alloy catalytic electrode with a three-dimensional porous structure, characterized in that: The steps include: 1) preparing an electrodeposition solution: dissolving two metal salts uniformly in one of water and an organic alcohol solution to obtain a salt alcohol solution and a salt water solution respectively; then adding the obtained salt water solution to the salt alcohol solution, stirring uniformly, to obtain a uniform and stable electrodeposition solution; 2) A two-electrode system is used, with a conductive substrate as the cathode, the cathode and the anode are immersed in an electrodeposition solution, electrochemical deposition is performed, and then washed and dried to obtain a self-supporting alloy catalytic electrode with a three-dimensional porous structure.
2. The preparation method according to claim 1, characterized in that: The conductive substrate is one of nickel mesh, nickel sheet, foam nickel, titanium mesh, titanium sheet, carbon cloth, carbon paper, foam copper, and graphene film.
3. The preparation method according to claim 1, characterized in that: The concentration of the organic salt alcohol solution is 0.5-2.5 mol / L.
4. The preparation method according to claim 1, characterized in that: The concentration of the saline solution is 0.01-0.05 mol / L.
5. The preparation method according to claim 1, characterized in that: The volume ratio of the saline alcohol solution to the saline solution is 1-10:
1.
6. The preparation method according to claim 1, characterized in that: The two metal salts in step 1) are specifically selected from two of nickel salts, iron salts, cobalt salts, manganese salts, zirconium salts, titanium salts, copper salts, cerium salts, tungstates, vanadates, and molybdates.
7. The preparation method according to claim 1, characterized in that: In the electrochemical deposition step, the applied current density is 0.1-3A / cm 2 , the deposition time is 90-600s.
8. The self-supporting alloy catalytic electrode prepared by the preparation method according to any one of claims 1 to 7, characterized in that: It includes a conductive substrate and an alloy particle deposition layer attached to the surface thereof, wherein the alloy particle deposition layer is distributed with macropores with a diameter of 8-50 μm, and at the same time, the surface and interior of the alloy particle deposition layer are uniformly distributed with accumulated pores with a diameter of 0.5-5 μm.
Citation Information
Cited By
Nickel-molybdenum alloy self-supporting catalytic electrode, preparation method thereof and application of nickel-molybdenum alloy self-supporting catalytic electrode in water electrolysis hydrogen production, carbon dioxide electrochemical reduction or nitrate electrochemical reduction
CN119465254A
Nickel-molybdenum alloy self-supporting catalytic electrode, preparation method thereof and application thereof in hydrogen production by water electrolysis, electrochemical reduction of carbon dioxide or electrochemical reduction of nitrate
CN119465254B
Non-noble metal-based self-supporting electrode, preparation method thereof and application of non-noble metal-based self-supporting electrode in efficient electrolyzed water
CN119800431A