Method for preparing thermosensitive block material by laser melting method

NiMn2O4 powder material with spinel structure was prepared by laser melting method, and thermal blocks were prepared on metal substrates, which solved the problems of performance and dimensional accuracy of the thermistor material in the prior art, and achieved high precision and high precision Performance production of thermistor components.

CN118894715AActive Publication Date: 2024-11-05NORTHWESTERN POLYTECHNICAL UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410933120.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

It is difficult to prepare high-performance NiMn2O4 materials suitable for thermistors in the prior art, and the commonly used methods are not suitable for the production of thermistor components with complex shapes and micrometer dimensional accuracy.

Method used

The NiO and MnO2 powder material reacted with oxalic acid solution by laser melting, and then annealed in a large atmosphere to form the NiMn2O4 powder material with spinel structure, and regulate the laser energy density on metal substrates such as stainless steel. Prepare heat-sensitive bulk materials.

Benefits of technology

It realizes the production of thermistor components with complex shapes and micrometer dimensional accuracy, and the material has good crystallinity, density and electrical properties, and is suitable for thermistor applications with high precision requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894715A_ABST
    Figure CN118894715A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing a thermosensitive block material by a laser melting method, which belongs to the field of functional oxide ceramic material preparation, and comprises the following steps: dissolving nickel oxide NiO and manganese dioxide MnO2 raw materials in an oxalic acid solution, drying to prepare a NiMn2O4 thermosensitive powder material, and annealing in an atmospheric environment to obtain a thermosensitive powder material with a spinel structure, and finally, melting the thermosensitive powder material laid on the substrate into the NiMn2O4 block material by using laser. Wherein the performance of the prepared NiMn2O4 block material can be regulated and controlled by controlling parameters such as energy density of the molten laser. The thermosensitive block material prepared by the method has the advantages of simple preparation process, high density, good electrical properties and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of functional oxide ceramic materials, and in particular relates to a method for preparing a thermosensitive bulk material by a laser melting method. Background Art

[0002] Negative temperature coefficient (NTC) thermistors have been extensively studied in recent decades due to their unique property of decreasing resistance as temperature increases. 3+ and Mn 4+ The material is widely used in aerospace, control, temperature monitoring and other industrial fields due to its high sensitivity to temperature changes, fast response speed and low cost. The simplest manganese-based transition metal oxide is NiMn2O4. In addition, the physical properties of manganese-based transition metal oxides can be changed by adding various metal ions such as cobalt, iron and zinc.

[0003] Currently, commonly used methods for synthesizing thermosensitive materials such as NiMn2O4 include solution method, solid phase sintering method, electric field assisted flash method and co-precipitation method, etc. Patent "CN109534412A" discloses a method for preparing three-dimensional porous NiMn2O4 using a self-sacrificial template method, but the NiMn2O4 prepared by this method is for use in supercapacitors and is not suitable for thermistors. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention proposes a method for preparing a thermosensitive bulk material by laser melting. The present invention uses a chemical solution and a laser melting method to prepare a NiMn2O4 powder material with a spinel structure using NiO powder material, MnO2 powder material and oxalic acid solution as raw materials, and performs a thermal annealing treatment in an atmospheric atmosphere. Finally, a NiMn2O4 thermosensitive bulk material is prepared on a substrate using different laser energy densities. The material has a simple preparation process, good crystallization, and good electrical properties.

[0005] In order to achieve the above object, the present invention is implemented by the following technical scheme: A method for preparing a thermosensitive block material by laser melting comprises the following steps:

[0006] Step 1) Put NiO and MnO2 powder raw materials into a beaker, then add alcohol and stir evenly;

[0007] Step 2) Slowly add oxalic acid solution into the beaker and continue stirring with a glass rod to prevent the generated gas from causing the material in the beaker to overflow;

[0008] Step 3) The beaker was placed in an ultrasonic cleaner and vibrated and stirred for 30 minutes to allow the powder raw material and oxalic acid to fully react;

[0009] Step 4) The beaker is then placed in a constant temperature water bath and heated until the solution in the beaker evaporates into a paste;

[0010] Step 5) drying the paste prepared in step 4 in a drying oven to obtain a precursor;

[0011] Step 6) annealing the precursor prepared in step 5) in an atmospheric atmosphere to obtain a NiMn2O4 thermosensitive powder material;

[0012] Step 7) setting the laser parameters of the laser melting equipment and determining the laser energy density that needs to be changed;

[0013] Step 8) Clean and wipe the substrate with alcohol, and then spread the NiMn2O4 powder material on the substrate;

[0014] Step 9) Turn on the laser instrument and set the laser beam to scan and melt the flat thermosensitive powder layer on the substrate to obtain a NiMn2O4 thermosensitive bulk material.

[0015] Furthermore, the purity of the NiO and MnO2 powder raw materials is both above 99.99%.

[0016] Furthermore, in step 6), the annealing temperature of the NiMn2O4 thermosensitive powder material is 830°C-900°C, and the annealing time is 100min-140min.

[0017] Furthermore, the NiMn2O4 thermosensitive powder material prepared in step 6) has a spinel structure.

[0018] Furthermore, the substrate material in step 8) is stainless steel, titanium alloy, aluminum alloy or other materials.

[0019] Furthermore, the laser parameters of the laser melting equipment are as follows: the laser power is not higher than 2000W, the laser scanning speed is not higher than 1cm / s, the scanning mode is unidirectional single scanning, and the powder laying thickness is 2mm.

[0020] Compared with the prior art, the present invention uses NiO, MnO2 powder materials and oxalic acid as raw materials to prepare NiMn2O4 powder materials, and then performs annealing treatment in the atmosphere to form NiMn2O4 powder materials with good crystal quality, and then obtains molten bulk NiMn2O4 materials on a stainless steel substrate by adjusting different laser energy densities. Its advantages are as follows:

[0021] 1. The present invention uses laser melting technology to manufacture thermistor components with complex shapes and micron dimensional accuracy, without the need for molds or tooling, to achieve free-form design and customized production. Moreover, through the study and analysis of samples, it is found that samples prepared under appropriate energy density usually have a smooth surface quality and high density.

[0022] 2. The laser melting method used in the present invention can prepare highly dense point-shaped, line-shaped and surface-shaped thermal block materials on a variety of metal substrate materials (including titanium alloy, stainless steel, aluminum alloy, etc.). In addition, the size of the thermal block material can achieve micron-level accuracy, which is suitable for manufacturing various thermistor components with high precision requirements on size and shape. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a simplified diagram of the preparation of materials on a stainless steel substrate by laser melting in an embodiment.

[0024] Figure 2 It is the XRD diagram of the NiMn2O4 thermosensitive bulk material prepared in Example 1-4.

[0025] Figure 3 This is a surface SEM image of the NiMn2O4 thermosensitive bulk material prepared in Example 1.

[0026] Figure 4 This is a surface SEM image of the NiMn2O4 thermosensitive bulk material prepared in Example 2.

[0027] Figure 5 This is a surface SEM image of the NiMn2O4 thermosensitive bulk material prepared in Example 3.

[0028] Figure 6 This is a surface SEM image of the NiMn2O4 thermosensitive bulk material prepared in Example 4.

[0029] Figure 7 The resistance-temperature curve and Ln(R / T)-1000 / T diagram of the NiMn2O4 thermosensitive bulk material prepared in Examples 1-4.

[0030] Figure 8 The aging performance diagram of the NiMn2O4 thermosensitive bulk material prepared in Examples 1-4 DETAILED DESCRIPTION

[0031] The present invention is further described in detail below with reference to the accompanying drawings and implementation examples. In order to better understand the method for preparing a thermosensitive bulk material by laser melting of the present invention, the specific steps of the present invention are briefly introduced first.

[0032] The method for preparing a thermosensitive bulk material by laser melting comprises the following steps:

[0033] Step 1) Select nickel oxide NiO and manganese dioxide MnO2 powder raw materials with a purity of more than 99.99%, put the NiO and MnO2 powder raw materials into a beaker, and then add alcohol and stir evenly.

[0034] Step 2) Slowly add oxalic acid solution into the beaker and continue stirring with a glass rod to prevent the generated gas from causing the material in the beaker to overflow;

[0035] Step 3) The beaker was placed in an ultrasonic cleaner and vibrated and stirred for 30 minutes to allow the powder raw material and oxalic acid to fully react;

[0036] Step 4) The beaker is then placed in a constant temperature water bath and heated until the solution in the beaker evaporates into a paste;

[0037] Step 5) drying the paste prepared in step 4 in a drying oven to obtain a precursor;

[0038] Step 6) annealing the precursor prepared in step 5) in an atmospheric atmosphere at a temperature of 830° C. to 900° C. for a time of 100 min to 140 min to obtain a NiMn2O4 thermosensitive powder material.

[0039] Step 7) Set the laser parameters of the laser melting equipment, the laser power is not higher than 2000W, the laser scanning speed is not higher than 1cm / s, the scanning mode is unidirectional single scanning, the powder thickness is 2mm, and the laser energy density that needs to be changed is determined. The laser energy density is the ratio of laser power to scanning speed, scanning spacing and powder thickness.

[0040] Step 8) Clean and wipe the substrate with alcohol, and then spread the NiMn2O4 powder material on the substrate. The substrate material is stainless steel, titanium alloy, aluminum alloy or other materials.

[0041] Step 9) Turn on the laser instrument and set the laser beam to scan and melt the flat thermosensitive powder layer on the substrate to obtain a NiMn2O4 thermosensitive bulk material.

[0042] The above briefly introduces the preparation method of the NiMn2O4 thermosensitive bulk material of the present invention. The following is a specific example and analysis of the prepared samples to verify the effect of the present invention.

[0043] Example 1

[0044] Using the chemical solution method, nickel oxide, manganese dioxide and oxalic acid solution are mixed, and after sufficient reaction, the precursor is dried. Then it is annealed in an atmosphere at 850°C for 120 minutes to obtain a NiMn2O4 powder material with a spinel structure. Finally, the NiMn2O4 powder material is spread on a stainless steel substrate and scanned and melted using a 1000W laser beam to obtain a NiMn2O4 thermosensitive bulk material.

[0045] Example 2

[0046] Using the chemical solution method, nickel oxide, manganese dioxide and oxalic acid solution are mixed, fully reacted, and then dried to obtain a precursor. Then, it is annealed in an atmosphere at 850°C for 120 minutes to obtain a NiMn2O4 powder material with a spinel structure. Finally, the NiMn2O4 powder material is spread on a stainless steel substrate and scanned and melted using a 1200W laser beam to obtain a NiMn2O4 thermosensitive bulk material.

[0047] Example 3

[0048] Using the chemical solution method, nickel oxide, manganese dioxide and oxalic acid solution are mixed, fully reacted, and then dried to obtain a precursor. Then it is annealed in an atmosphere at 850°C for 120 minutes to obtain a NiMn2O4 powder material with a spinel structure. Finally, the NiMn2O4 powder material is spread on a stainless steel substrate and scanned and melted using a 1500W laser beam to obtain a NiMn2O4 thermosensitive bulk material.

[0049] Example 4

[0050] Using the chemical solution method, nickel oxide, manganese dioxide and oxalic acid solution are mixed, and after sufficient reaction, the precursor is dried. Then it is annealed in an atmosphere at 850°C for 120 minutes to obtain a NiMn2O4 powder material with a spinel structure. Finally, the NiMn2O4 powder material is spread on a stainless steel substrate and scanned and melted using a 2000W laser beam to obtain a NiMn2O4 thermosensitive bulk material.

[0051] The four samples prepared in Examples 1-4 were analyzed using an X-ray diffractometer and a scanning electron microscope. Figure 2-7 and Table 1.

[0052] Figure 2 The results show that the peaks of the four samples are all spinel phase NiMn2O4 with good crystallinity, and no diffraction peaks of other impurity phases are observed. The main diffraction peak orientations are (311), (400), (422), (511), and (440), and the characteristic peak (400) is the strongest when the laser power is 2000W.

[0053] Figure 3-6 The results show that when the laser power is 1500W, that is, the sample surface corresponding to Example 3 is smooth and has no holes, and has higher density. However, defects such as holes and cracks appear on the surfaces of other samples. The result is that when the laser power is too low, the amount of liquid formed by the melting of the powder material is reduced, so that the concentration of the liquid-solid mixture becomes very high, which hinders the flow of the liquid and the rearrangement of the particles. Therefore, adjacent spherical powder materials are not effectively combined, and the lack of melt holes and spheroidization are prone to occur during the scanning process; in addition, excessive laser power will lead to a large temperature gradient. The extremely high temperature gradient and the thermal shock effect of the laser will cause internal stress in the sample, causing cracks on the sample surface and reducing the density.

[0054] Figure 7 The results in Table 1 show that the resistance values ​​of the four samples decrease with increasing temperature, which is consistent with the characteristics of NTC thermistors. The Ln(R) of the four samples is linearly related to 1000 / T, showing a typical small polaron hopping mechanism. In addition, the B value is the largest when the laser power is 1500W, indicating that its electrical performance is the best. In general, the electrical performance of the samples is enhanced.

[0055] Figure 8 The aging performance parameter diagram of four samples annealed at 125°C for 600h. It can be obtained that the aging performance is best when the laser power is 1500W, which is only about 10%. The poor aging performance of the other three samples can be attributed to the poor densification of their samples. The dense microstructure can stabilize the distribution of cations and inhibit the oxidation and diffusion of cation vacancies between grains and grain boundaries. The poor microstructure of the other three samples will enhance the atmospheric oxygen adsorption of the material, and oxygen adsorption will cause the Mn on the tetrahedron to 2+ It is easily oxidized to Mn 3+ , making the structure of cation distribution unstable and easier to migrate, resulting in poor aging performance.

[0056] The method of the present invention can be used to obtain bulk NiMn2O4 thermosensitive material; the obtained sample has good crystallinity, good density and excellent electrical properties.

[0057] Table 1 Electrical performance parameters of NiMn2O4 thermosensitive bulk materials prepared in Examples 1-4

[0058] Power / W <![CDATA[R 315 (MΩ)]]> <![CDATA[R 345 (MΩ)]]> <![CDATA[B 315 / 345 (K)]]> <![CDATA[E a (eV)]]> 1000 5.5 2.37 3049.6 0.6746 1200 4.95 2.18 29707. 0.6571 1500 6.52 2.55 3400.7 0.7523 2000 1.76 0.72 3237.9 0.7162

[0059] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A method for preparing a thermosensitive bulk material by laser melting, characterized in that: The following steps are involved: Step 1) Put NiO and MnO2 powder raw materials into a beaker, then add alcohol and stir evenly; Step 2) Slowly add oxalic acid solution into the beaker and continue stirring with a glass rod; Step 3) The beaker was placed in an ultrasonic cleaner for vibration and stirring for 30 minutes to allow the powder raw material and oxalic acid to fully react; Step 4) The beaker is then placed in a constant temperature water bath and heated until the solution in the beaker evaporates into a paste; Step 5) drying the paste prepared in step 4 in a drying oven to obtain a precursor; Step 6) annealing the precursor prepared in step 5) in an atmospheric atmosphere to obtain a NiMn2O4 thermosensitive powder material; Step 7) setting the laser parameters of the laser melting equipment and determining the laser energy density that needs to be changed; Step 8) Clean and wipe the substrate with alcohol, and then spread the NiMn2O4 powder material on the substrate; Step 9) Turn on the laser instrument and set the laser beam to scan and melt the flat thermosensitive powder layer on the substrate to obtain a NiMn2O4 thermosensitive bulk material.

2. The method for preparing a thermosensitive bulk material by laser melting according to claim 1, characterized in that: The purity of the NiO and MnO2 powder raw materials is both above 99.99%.

3. The method for preparing a thermosensitive bulk material by laser melting according to claim 1, characterized in that: In the step 6), the annealing temperature of the NiMn2O4 thermosensitive powder material is 830°C-900°C, and the annealing time is 100min-140min.

4. The method for preparing a thermosensitive bulk material by laser melting according to claim 3, characterized in that: The NiMn2O4 thermosensitive powder material prepared in step 6) has a spinel structure.

5. The method for preparing a thermosensitive bulk material by laser melting according to claim 1, characterized in that: The substrate material in step 8) is stainless steel, or titanium alloy, or aluminum alloy.

6. The method for preparing a thermosensitive bulk material by laser melting according to claim 1, characterized in that: The laser parameters of the laser melting equipment are as follows: the laser power is not higher than 2000W, the laser scanning speed is not higher than 1cm / s, the scanning mode is unidirectional single scanning, and the powder laying thickness is 2mm.

Citation Information

Patent Citations

  • Ntc thermistor porcelain, process for producing NTC thermistor porcelain, and NTC thermistor

    CN102017023A

  • Preparation method of quasicrystal block

    CN102443799A

  • Novel Ni-Mn-Ga resin based composite material, and preparation method thereof

    CN102924875A

  • Preparation process of high-precision NTC thermal sensitive ceramic

    CN109020500A

  • Method for preparing magnesium silicide thermoelectric material block, device and thermoelectric material block

    CN110729391A