Nanocrystalline high-strength alumina ceramic substrate material and preparation method thereof
By optimizing the particle size matching and dispersant of alumina powder, combining sintering aids and rare earth additives, reducing the sintering temperature, the problem of insufficient mechanical properties of alumina ceramic substrate materials is solved, and high-strength and high-density nanocrystalline alumina is achieved Ceramic substrate preparation.
Patent Information
- Application Number
- CN202411134136.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The grain size of the existing alumina ceramic substrate materials is difficult to refine to the nanoscale. The high sintering temperature leads to excessive growth of grains, insufficient mechanical properties, and nano-scale alumina powders are prone to agglomeration and dispersion, and have low density.
Nano-grade alumina powder is used to design powder matching with different particle size ranges and the synergistic effect of multiple dispersants, combining the components of the sintering additives and the powder particle size ratio to reduce the sintering temperature, and using rare earth additives to inhibit grain growth. Ball mill dispersion process and casting forming technology form high-density alumina ceramic substrate.
The bending strength of the alumina ceramic substrate is significantly improved, with a grain size of 100-300nm, a density higher than 3.95g/cm3, a low surface roughness, a small warpage, and a bending strength of more than 600MPa, solving the insufficient mechanical performance The problem.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic materials, and specifically discloses a nanocrystalline high-strength alumina ceramic substrate material and a preparation method thereof. Background Art
[0002] With the development of information technology, the electronics industry has become one of the most dynamic, innovative and important industries in the world economy today. Electronic packaging technology plays a vital role in the electronics industry and is the guarantee for the normal and stable operation of semiconductor chips. Among them, electronic packaging materials are the top priority of electronic packaging technology. Ceramic material packaging has good chemical stability, high thermal conductivity, high mechanical strength, low thermal expansion coefficient, low dielectric constant and low dielectric loss, and has attracted much attention. Alumina ceramic packaging substrate materials have excellent electrical properties, mechanical properties, and chemical stability. They are superior to most oxide ceramics in mechanical, thermal, electrical and other physical properties. In addition, the raw material source is abundant and the cost is low. It is the most commonly used substrate material in the integrated circuits of the current electronics industry, accounting for more than 80% of the total ceramic substrate materials. At present, alumina ceramic substrates are widely used in thick film circuits, thin film circuits, hybrid integrated circuits, multi-chip components, and high-power IGBT modules.
[0003] With the development of 5G and 6G communication technologies, and the rise of third-generation semiconductors such as GaN, AlN, and SiC, power devices have developed rapidly, and the demand for alumina ceramic packaging has surged. In some harsh and severe environments, such as aerospace, space exploration, and deep-sea drilling, higher performance requirements are also put forward for alumina packaging ceramics. In order to meet the requirements of high power, high-density packaging and long life of devices, alumina substrates need to have higher physical and mechanical properties, especially higher requirements for the bending strength of alumina substrate materials. The performance of the currently used medium-grained (1-4μm) alumina ceramic materials can no longer fully meet the needs of the new generation of electronic packaging technology. Refinement is the main way to improve the performance of alumina substrates. The microstructure of fine-grained alumina ceramics is more uniform and the mechanical properties are significantly improved. However, most of the existing relatively mature technologies can only refine the alumina grain size to the submicron level (0.8-1.0μm), and cannot refine the grains to the nanometer level below 0.5μm. Because alumina generally has low sintering activity and high sintering temperature, sintering at too high a temperature will lead to excessive grain growth, resulting in weakened mechanical properties. In addition, the problems of easy agglomeration, difficult dispersion, and low sintering density of nano-alumina powder have not been solved.
[0004] Therefore, the preparation of high-performance nanocrystalline alumina substrate materials faces severe challenges. Summary of the invention
[0005] In view of the above-mentioned deficiencies, the present invention adopts nano-scale alumina powder, and solves the problems of low strength and insufficient mechanical properties of medium-grained alumina ceramic substrates by designing and optimizing the combination of powders in different particle size ranges. The present application utilizes the synergistic effect of multiple dispersants and surfactants to solve the problems of easy agglomeration and difficulty in dispersion of nano-grains. The present application effectively reduces the sintering temperature of alumina ceramics by designing the composition of sintering aids and the powder particle size ratio. Under the premise of ensuring the sintering density of the material, the sintering temperature is effectively reduced, and the growth of nano-grains is effectively inhibited, thereby improving the strength of the alumina ceramic substrate material. The alumina substrate material obtained in the present application has a grain size of 100-300nm and a density of ≥3.95g / cm 3 , surface roughness ≤0.2μm, warpage ≤0.1mm, bending strength ≥600MPa, no cracking, breakage and other appearance defects.
[0006] The present invention is achieved by the following technical means:
[0007] The present invention first discloses a method for preparing an alumina ceramic substrate material, comprising:
[0008] (1) Batching and mixing
[0009] Weigh 3-6wt% of sintering aid, 0.5-2.0wt% of rare earth additive and the balance of alumina powder, mix them and add them into a ball mill to obtain a first mixture;
[0010] Take the first mixture, add a solvent and a dispersant, add 40-100 ml of the solvent and 30-80 ml of the dispersant to every 100 g of the first mixture, to obtain a second mixture;
[0011] The second mixture is added to alumina ceramic grinding balls and ground and dispersed for 10-15 hours, the mass ratio of the grinding balls to the second mixture is 2:1-5:1, and the ball mill speed is 600-1000 r / min to obtain a dispersed slurry;
[0012] Add 10-20% of the first mixture by mass percentage of the binder to the dispersed slurry, then add 5-20% of the first mixture by mass percentage of the plasticizer, perform secondary ball milling, the speed is 600-800r / min, the ball milling time is 8-15h, and finally the speed is reduced to 200-400r / min and mixed for 1-3h. When pouring out the slurry, filter the slurry with a 200-mesh screen to remove the binder blocks, large particles of powder and other residues to obtain a stable and uniform casting slurry.
[0013] (2) Defoaming
[0014] The obtained casting slurry is defoamed on a vacuum defoamer with a vacuum degree of less than -0.1 MPa, a temperature controlled at 30-45°C, and a time of 1-3 hours. The viscosity of the defoamed slurry obtained is 2000-4000 mPa·s.
[0015] (3) Tape casting
[0016] The defoamed slurry is cast on a tape casting machine to obtain a green sheet. The temperature of the tape casting is 50-90°C, the speed of the tape casting is 0.2-0.5m / min, and the scraper gap is 300-600μm. After that, it is dried at 80-150°C for 1-3h to obtain an alumina substrate green sheet.
[0017] (4) Debonding
[0018] The formed green sheet is placed in a debinding furnace for debinding, the debinding temperature is 700-800°C, the debinding time is 3-6h, nitrogen or argon conditions, the gas flow rate is 5-10L / min. The heating rate is 0.5-1.0°C / min from room temperature to 300°C, and the heating rate is 1.0-1.5°C / min from 300°C to debinding temperature to obtain debinding alumina material.
[0019] (5) Sintering
[0020] The debinding alumina material is transferred into a low-pressure sintering furnace for pressure sintering, and the temperature is increased to 1320-1420°C at a heating rate of 1-3°C / min, the sintering time is 2-3h, the sintering atmosphere is nitrogen or argon, and the sintering pressure is 2-6MPa, and finally an alumina ceramic substrate material is obtained.
[0021] Furthermore, the alumina powder in step (1) is nano and submicron alumina powder with a mass fraction of >99.9wt%, wherein:
[0022] Powder with a particle size of 40-80nm accounts for 5-8wt%, powder with a particle size of 80-150nm accounts for 20-25wt%, powder with a particle size of 150-200nm accounts for 30-40wt%, powder with a particle size of 200-250nm accounts for 15-24wt%, and the remainder is powder with a particle size of 250-300nm.
[0023] Furthermore, the rare earth additive is prepared by mixing CeO2 and La2O3 with a particle size of 50-100 nm, and the mass ratio of CeO2 to La2O3 is 2:1-4:1.
[0024] Further, the solvent is prepared by mixing ethyl acetate, butyl acetate, acetone and anhydrous ethanol, wherein:
[0025] Ethyl acetate 30-40wt%, butyl acetate 20-30wt%, acetone 10-20wt%, and the balance is anhydrous ethanol.
[0026] Furthermore, the dispersant in step (1) is prepared by mixing triolein, castor oil and polymethacrylic acid, wherein:
[0027] 30-40wt% triolein, 20-30wt% castor oil, and the balance is polymethacrylic acid.
[0028] Furthermore, in step (1), the binder is polyvinyl butyral, and the plasticizer is dibutyl phthalate.
[0029] Furthermore, in step (1), the second mixture is added with alumina ceramic grinding balls including grinding balls with diameters of 1 mm, 2 mm, 4 mm and 6 mm, wherein:
[0030] Grinding balls with a diameter of 1 mm account for 10-20wt%, grinding balls with a diameter of 2 mm account for 30-40wt%, grinding balls with a diameter of 4 mm account for 20-30wt%, and the remainder is grinding balls with a diameter of 6 mm.
[0031] Furthermore, the sintering aid used in the sintering of step (5) is a mixture of CaO+SiO2+MgO+B2O3, wherein:
[0032] The particle size of CaO powder is 50-100nm, accounting for 10-20wt%; the particle size of SiO2 powder is 50-100nm, accounting for 30-40wt%; the particle size of MgO powder is 50-100nm, accounting for 10-20wt%; the particle size of B2O3 powder is 50-100nm, and the rest is B2O3 powder.
[0033] The invention also discloses an alumina ceramic substrate material prepared according to any one of the above preparation methods.
[0034] Furthermore, the grain size of the alumina substrate material is 100-300nm, and the density is ≥3.95g / cm 3 , surface roughness ≤0.2μm, warpage ≤0.1mm, bending strength ≥600MPa.
[0035] The beneficial effects of the present invention are:
[0036] The present invention adopts nano-alumina powders of different particle size ranges to prepare nanocrystalline ceramic substrate materials, and designs the composition ratio and content of multiple dispersants, and effectively overcomes the agglomeration problem of nano-powders with the ball milling dispersion process, significantly improving the dispersion effect of nano powders, and further designing and regulating the composition ratio and particle size range of sintering aids, effectively reducing the sintering temperature of alumina ceramics, and supplemented by the grain growth inhibition effect of rare earth oxides, effectively inhibiting the growth behavior of nano alumina grains during the sintering process, and finally preparing an alumina ceramic substrate material with excellent performance, significantly improving the flexural strength of alumina ceramic materials. The performance of the alumina substrate material obtained by the present invention is compared with the performance of conventional medium-grained alumina as shown in the following table, and it can be seen that the flexural strength, density, warpage, etc. of the alumina material in this application are significantly improved. DETAILED DESCRIPTION
[0037] For ease of understanding of the present invention, the present invention will be described more fully below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0039] Example 1
[0040] A high-strength ultra-nanocrystalline alumina ceramic substrate material and a preparation method thereof include:
[0041] The nanometer and submicron aluminum oxide powder with a mass fraction higher than 99.9wt% is used, among which the powder with a particle size of 40-80nm is 5wt%, the powder with a particle size of 80-150nm is 25wt%, the powder with a particle size of 150-200nm is 40wt%, the powder with a particle size of 200-250nm is 15wt%, and the powder with a particle size of 250-300nm is 15wt%.
[0042] CaO+SiO2+MgO+B2O3 are used as sintering aids, wherein CaO powder is 50-100nm, SiO2 powder is 50-100nm, MgO powder is 50-100nm, and B2O3 powder is 50-100nm, wherein CaO powder is 20wt%, MgO powder is 20wt%, SiO2 powder is 40wt%, and B2O3 powder is 20wt%.
[0043] CeO2 and La2O3 with a particle size of 50-100 nm are used as rare earth additives, wherein the mass ratio of CeO2 to La2O3 is 2:1.
[0044] The solvents used are ethyl acetate, butyl acetate, acetone and anhydrous ethanol, wherein ethyl acetate is 40wt%, butyl acetate is 30wt%, acetone is 10wt% and anhydrous ethanol is 20wt%.
[0045] The dispersants used are triolein, castor oil and polymethacrylic acid, wherein the triolein is 30 wt %, the castor oil is 30 wt % and the polymethacrylic acid is 40 wt %.
[0046] The adhesive used is polyvinyl butyral, and the plasticizer used is dibutyl phthalate.
[0047] (1) Batching and mixing
[0048] Weigh alumina powder, sintering aid and rare earth additive, wherein the content of solvent is 3wt%, the content of rare earth additive is 1.0wt%, and the content of alumina powder is 96wt%. Add the weighed alumina powder, solvent and rare earth additive into a ball mill, and add solvent, the amount of solvent added is 100g (solid powder): 60ml. Add dispersant, the amount of dispersant added is 100g (solid powder): 60ml. Then add alumina ceramic grinding balls (10wt% for 1mm diameter grinding balls, 40wt% for 2mm diameter grinding balls, 30wt% for 4mm diameter grinding balls, 20wt% for 6mm diameter grinding balls), the mass ratio of grinding balls to solid powder is 3:1, the ball mill speed is 800r / min, and the ball milling dispersion is carried out for 10h to give the slurry fluidity.
[0049] Add 15% of the solid powder mass binder to the slurry after ball milling, and then add 10% of the solid powder mass plasticizer, and perform secondary ball milling at a speed of 600r / min for 10h, and finally reduce the speed to 200r / min and mix for 2h. When pouring out the slurry, filter the slurry with a 200-mesh screen to remove the binder blocks, large particles of powder and other residues to obtain a stable and uniform casting slurry.
[0050] (2) Defoaming
[0051] The obtained slurry was defoamed in a vacuum defoamer with a vacuum degree of less than -0.1 MPa and a temperature controlled at 35°C for 1 hour. The viscosity of the final slurry was about 3500 mPa·s.
[0052] (3) Tape casting
[0053] The defoamed slurry was cast on a tape casting machine to obtain a green sheet. The casting temperature was 65°C, the casting speed was 0.3 m / min, and the scraper gap was 450 μm. After that, it was dried at 120°C for 1.5 hours to obtain an alumina substrate green sheet.
[0054] (4) Debonding
[0055] The green sheet after tape casting is placed in a debinding furnace for debinding, the debinding temperature is 700℃, the debinding time is 5h, nitrogen or argon gas conditions, gas flow rate is 5L / min. The heating rate is 0.5℃ / min from room temperature to 300℃, and the heating rate is 1.0℃ / min from 300℃ to 700℃.
[0056] (5) Sintering
[0057] The debinded alumina material was transferred to a low-pressure sintering furnace for pressure sintering, and the temperature was raised to 1400°C at a heating rate of 2°C / min, the sintering time was 2h, the sintering atmosphere was nitrogen or argon, and the sintering pressure was 3MPa. Finally, a high-performance alumina substrate material was obtained.
[0058] The alumina substrate material obtained in this example has a grain size of 200-400nm and a density of 3.99g / cm 3 , density 99%, surface roughness ≤0.2μm, warpage ≤0.1mm, bending strength 640MPa, no cracking, breakage and other appearance defects.
[0059] Example 2
[0060] A high-strength ultra-nanocrystalline alumina ceramic substrate material and a preparation method thereof include:
[0061] The nanometer and submicron aluminum oxide powder with a mass fraction higher than 99.9wt% is used, among which the powder with a particle size of 40-80nm is 5wt%, the powder with a particle size of 80-150nm is 25wt%, the powder with a particle size of 150-200nm is 40wt%, the powder with a particle size of 200-250nm is 15wt%, and the powder with a particle size of 250-300nm is 15wt%.
[0062] CaO+SiO2+MgO+B2O3 are used as sintering aids, wherein CaO powder is 50-100nm, SiO2 powder is 50-100nm, MgO powder is 50-100nm, and B2O3 powder is 50-100nm, wherein CaO powder is 20wt%, MgO powder is 20wt%, SiO2 powder is 40wt%, and B2O3 powder is 20wt%.
[0063] CeO2 and La2O3 with a particle size of 50-100 nm are used as rare earth additives, wherein the mass ratio of CeO2 to La2O3 is 2:1.
[0064] The solvents used are ethyl acetate, butyl acetate, acetone and anhydrous ethanol, wherein ethyl acetate is 40wt%, butyl acetate is 30wt%, acetone is 10wt% and anhydrous ethanol is 20wt%.
[0065] The dispersants used are triolein, castor oil and polymethacrylic acid, wherein the triolein is 30 wt %, the castor oil is 30 wt % and the polymethacrylic acid is 40 wt %.
[0066] The adhesive used is polyvinyl butyral, and the plasticizer used is dibutyl phthalate.
[0067] (1) Batching and mixing
[0068] Weigh alumina powder, sintering aid and rare earth additive, wherein the content of solvent is 6wt%, the content of rare earth additive is 1.2wt%, and the content of alumina powder is 93.8wt%. Add the weighed alumina powder, solvent and rare earth additive into a ball mill, and add solvent, the amount of solvent added is 100g (solid powder): 60ml. Add dispersant, the amount of dispersant added is 100g (solid powder): 60ml. Then add alumina ceramic grinding balls (10wt% for 1mm diameter grinding balls, 40wt% for 2mm diameter grinding balls, 30wt% for 4mm diameter grinding balls, 20wt% for 6mm diameter grinding balls), the mass ratio of grinding balls to solid powder is 3:1, the ball mill speed is 800r / min, and the ball milling dispersion is carried out for 10h to give the slurry fluidity.
[0069] Add 15% of the solid powder mass binder to the slurry after ball milling, and then add 10% of the solid powder mass plasticizer, and perform secondary ball milling at a speed of 600r / min for 10h, and finally reduce the speed to 200r / min and mix for 2h. When pouring out the slurry, filter the slurry with a 200-mesh screen to remove the binder blocks, large particles of powder and other residues to obtain a stable and uniform casting slurry.
[0070] (2) Defoaming
[0071] The obtained slurry was defoamed in a vacuum defoamer with a vacuum degree of less than -0.1 MPa and a temperature controlled at 35°C for 1 hour. The viscosity of the final slurry was about 3500 mPa·s.
[0072] (3) Tape casting
[0073] The defoamed slurry was cast on a tape casting machine to obtain a green sheet. The casting temperature was 65°C, the casting speed was 0.3 m / min, and the scraper gap was 450 μm. After that, it was dried at 120°C for 1.5 hours to obtain an alumina substrate green sheet.
[0074] (4) Debonding
[0075] The green sheet after tape casting is placed in a debinding furnace for debinding, the debinding temperature is 700℃, the debinding time is 5h, nitrogen or argon gas conditions, gas flow rate is 5L / min. The heating rate is 0.5℃ / min from room temperature to 300℃, and the heating rate is 1.0℃ / min from 300℃ to 700℃.
[0076] (5) Sintering
[0077] The debinded alumina material was transferred to a low-pressure sintering furnace for pressure sintering, and the temperature was raised to 1320°C at a heating rate of 2°C / min, the sintering time was 2h, the sintering atmosphere was nitrogen or argon, and the sintering pressure was 5MPa. Finally, a high-performance alumina substrate material was obtained.
[0078] The alumina substrate material obtained in this example has a grain size of 100-300nm and a density of 3.95g / cm 3 , density 98.5%, surface roughness ≤0.2μm, warpage ≤0.1mm, bending strength 610MPa, no cracking, breakage and other appearance defects.
[0079] Example 3
[0080] A high-strength ultra-nanocrystalline alumina ceramic substrate material and a preparation method thereof include:
[0081] The nanometer and submicron aluminum oxide powder with a mass fraction higher than 99.9wt% is used, of which the powder with a particle size of 40-80nm is 8wt%, the powder with a particle size of 80-150nm is 20wt%, the powder with a particle size of 150-200nm is 40wt%, the powder with a particle size of 200-250nm is 24wt%, and the powder with a particle size of 250-300nm is 8wt%.
[0082] CaO+SiO2+MgO+B2O3 are used as sintering aids, wherein CaO powder is 50-100nm, SiO2 powder is 50-100nm, MgO powder is 50-100nm, and B2O3 powder is 50-100nm, wherein CaO powder is 20wt%, MgO powder is 20wt%, SiO2 powder is 40wt%, and B2O3 powder is 20wt%.
[0083] CeO2 and La2O3 with a particle size of 50-100 nm are used as rare earth additives, wherein the mass ratio of CeO2 to La2O3 is 2:1.
[0084] The solvents used are ethyl acetate, butyl acetate, acetone and anhydrous ethanol, wherein ethyl acetate is 40wt%, butyl acetate is 30wt%, acetone is 10wt% and anhydrous ethanol is 20wt%.
[0085] The dispersants used are triolein, castor oil and polymethacrylic acid, wherein the triolein is 30 wt %, the castor oil is 30 wt % and the polymethacrylic acid is 40 wt %.
[0086] The adhesive used is polyvinyl butyral, and the plasticizer used is dibutyl phthalate.
[0087] (1) Batching and mixing
[0088] Weigh alumina powder, sintering aid and rare earth additive, wherein the content of solvent is 5wt%, the content of rare earth additive is 1.5wt%, and the content of alumina powder is 94.5wt%. Add the weighed alumina powder, solvent and rare earth additive into a ball mill, and add solvent, the amount of solvent added is 100g (solid powder): 100ml. Add dispersant, the amount of dispersant added is 100g (solid powder): 80ml. Then add alumina ceramic grinding balls (10wt% for 1mm diameter grinding balls, 40wt% for 2mm diameter grinding balls, 30wt% for 4mm diameter grinding balls, 20wt% for 6mm diameter grinding balls), the mass ratio of grinding balls to solid powder is 3:1, the ball mill speed is 800r / min, and the ball milling dispersion is carried out for 10h to give the slurry fluidity.
[0089] Add 15% of the solid powder mass binder to the slurry after ball milling, and then add 10% of the solid powder mass plasticizer, and perform secondary ball milling at a speed of 600r / min for 10h, and finally reduce the speed to 200r / min and mix for 2h. When pouring out the slurry, filter the slurry with a 200-mesh screen to remove the binder blocks, large particles of powder and other residues to obtain a stable and uniform casting slurry.
[0090] (2) Defoaming
[0091] The obtained slurry was defoamed in a vacuum defoamer with a vacuum degree of less than -0.1 MPa and a temperature controlled at 35°C for 1 h. The viscosity of the final slurry was about 4000 mPa·s.
[0092] (3) Tape casting
[0093] The defoamed slurry was cast on a tape casting machine to obtain a green sheet. The casting temperature was 65°C, the casting speed was 0.3 m / min, and the scraper gap was 450 μm. After that, it was dried at 120°C for 1.5 hours to obtain an alumina substrate green sheet.
[0094] (4) Debonding
[0095] The green sheet after tape casting is placed in a debinding furnace for debinding, the debinding temperature is 700℃, the debinding time is 5h, nitrogen or argon gas conditions, gas flow rate is 5L / min. The heating rate is 0.5℃ / min from room temperature to 300℃, and the heating rate is 1.0℃ / min from 300℃ to 700℃.
[0096] (5) Sintering
[0097] The debinded alumina material was transferred to a low-pressure sintering furnace for pressure sintering, and the temperature was raised to 1380°C at a heating rate of 2°C / min, the sintering time was 2h, the sintering atmosphere was nitrogen or argon, and the sintering pressure was 5MPa. Finally, a high-performance alumina substrate material was obtained.
[0098] The alumina substrate material obtained in this example has a grain size of 100-500nm and a density of 3.95g / cm 3 , density is higher than 98.5%, surface roughness ≤0.2μm, warpage ≤0.1mm, bending strength 630MPa, no cracking, breakage and other appearance defects.
[0099] Table 1
[0100]
[0101] According to the results in Table 1, the preparation process of the present invention reduces the sintering temperature of the alumina ceramic substrate material to below 1400°C. The significantly reduced sintering temperature effectively reduces the growth trend of nano-alumina grains during the sintering process, making the alumina grain size below 500nm, while not reducing the sintering density of the alumina ceramic (above 98.5%). The surface roughness of the alumina ceramic substrate obtained in the present invention is less than 0.2μm, which is significantly lower than that of the usual alumina substrate (usually above 0.35μm), and the sintering warpage of the ceramic substrate is significantly reduced. At the same time, the present invention greatly improves the flexural strength of the alumina ceramic substrate material to above 600MPa, which is much higher than the usual alumina ceramic material.
[0102] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0103] The above-described embodiments only express several implementation methods of the present invention, which are convenient for understanding the technical solutions of the present invention in detail, but they cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided by the present invention are all within the protection scope of the attached claims described in the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the contents of the attached claims, and the description can be used to interpret the contents of the claims.
Claims
1. A method for preparing an alumina ceramic substrate material, comprising: (1) Batching and mixing Weigh 3-6wt% of sintering aid, 0.5-2.0wt% of rare earth additive and the balance of alumina powder, mix them and add them into a ball mill to obtain a first mixture; Take the first mixture, add a solvent and a dispersant, add 40-100 ml of the solvent and 30-80 ml of the dispersant to every 100 g of the first mixture, to obtain a second mixture; The second mixture is added to alumina ceramic grinding balls and ground and dispersed for 10-15 hours, the mass ratio of the grinding balls to the second mixture is 2:1-5:1, and the ball mill speed is 600-1000 r / min to obtain a dispersed slurry; Add 10-20% of the first mixture by mass percentage of the adhesive to the dispersed slurry, then add 5-20% of the first mixture by mass percentage of the plasticizer, perform secondary ball milling, the speed is 600-800r / min, the ball milling time is 8-15h, and finally the speed is reduced to 200-400r / min and mixed for 1-3h, and the ground slurry is passed through a 200-mesh screen to obtain a casting slurry; (2) Defoaming The casting slurry is defoamed on a vacuum defoamer with a vacuum degree of less than -0.1MPa and a temperature of 30-45°C for 1-3h to obtain a defoamed slurry; (3) Tape casting The defoamed slurry is tape-casted on a tape-casting machine to obtain a green sheet, the tape-casting temperature is 50-90° C., the tape-casting speed is 0.2-0.5 m / min, and the scraper gap is 300-600 μm to obtain a formed green sheet; (4) Debonding The formed green sheet is placed in a debinding furnace for debinding, the debinding temperature is 700-800°C, the debinding time is 3-6h, nitrogen or argon conditions, the gas flow rate is 5-10L / min, the heating rate is 0.5-1.0°C / min from room temperature to 300°C, and the heating rate is 1.0-1.5°C / min from 300°C to the debinding temperature to obtain a debinding alumina material; (5) Sintering The debinding alumina material is transferred into a low-pressure sintering furnace for pressure sintering, and the temperature is increased to 1320-1420°C at a heating rate of 1-3°C / min, the sintering time is 2-3h, the sintering atmosphere is nitrogen or argon, and the sintering pressure is 2-6MPa, and finally an alumina ceramic substrate material is obtained.
2. The preparation method according to claim 1, wherein: The alumina powder in step (1) is nano and submicron alumina powder with a mass fraction of >99.9wt%, comprising: Powder with a particle size of 40-80nm accounts for 5-8wt%, powder with a particle size of 80-150nm accounts for 20-25wt%, powder with a particle size of 150-200nm accounts for 30-40wt%, powder with a particle size of 200-250nm accounts for 15-24wt%, and the remainder is powder with a particle size of 250-300nm.
3. The preparation method according to claim 1, wherein: The rare earth additive in step (1) is prepared by mixing CeO2 and La2O3 with a particle size of 50-100 nm, and the mass ratio of CeO2 to La2O3 is 2:1-4:
1.
4. The preparation method according to claim 1, wherein: The solvent in step (1) is prepared by mixing ethyl acetate, butyl acetate, acetone and anhydrous ethanol, wherein: Ethyl acetate 30-40wt%, butyl acetate 20-30wt%, acetone 10-20wt%, and the balance is anhydrous ethanol.
5. The preparation method according to claim 1, wherein: The dispersant in step (1) is prepared by mixing triolein, castor oil and polymethacrylic acid, wherein: 30-40wt% triolein, 20-30wt% castor oil, and the balance is polymethacrylic acid.
6. The preparation method according to claim 1, wherein: In step (1), the binder is polyvinyl butyral and the plasticizer is dibutyl phthalate.
7. The preparation method according to claim 1, wherein: Step (1) The second mixture is added with alumina ceramic grinding balls including grinding balls with diameters of 1 mm, 2 mm, 4 mm and 6 mm, wherein: Grinding balls with a diameter of 1 mm account for 10-20wt%, grinding balls with a diameter of 2 mm account for 30-40wt%, grinding balls with a diameter of 4 mm account for 20-30wt%, and the remainder is grinding balls with a diameter of 6 mm.
8. The preparation method according to claim 1, wherein: The sintering aid used in the sintering of step (5) is a mixture of CaO+SiO2+MgO+B2O3, wherein: The particle size of CaO powder is 50-100nm, accounting for 10-20wt%; the particle size of SiO2 powder is 50-100nm, accounting for 30-40wt%; the particle size of MgO powder is 50-100nm, accounting for 10-20wt%; the particle size of B2O3 powder is 50-100nm, and the rest is B2O3 powder.
9. An alumina ceramic substrate material obtained according to the preparation method according to any one of claims 1 to 8.
10. The aluminum oxide substrate material according to claim 9, wherein: The alumina ceramic substrate material has a grain size of 100-300nm and a density of ≥3.95g / cm 3 , surface roughness ≤0.2μm, warpage ≤0.1mm, bending strength ≥600MPa.
Citation Information
Patent Citations
Low-temperature co-fired ceramic tape casting material and preparing method and application thereof
CN103482985A
LED (Light-Emitting Diode) substrate material and preparation method thereof
CN103601476A
Preparation method for non-water-based high-purity nanoscale aluminum oxide ceramics
CN104987050A
Laminated electronic component casting slurry and preparation method thereof
CN107619285A
Preparation method for laminated aluminum matrix composite material without residual pyrolytic carbon
CN107825776A
Cited By
Lanthanum trioxide reinforced and toughened aluminum oxide ceramic and preparation method of aluminum oxide ceramic
CN121225990A
Preparation method of 96 aluminum oxide ceramic substrate
CN121362033A
Preparation method of aluminum oxide substrate
CN121470936A
Preparation method of high-strength aluminum oxide ceramic substrate
CN121651886A