Magnetic antibacterial bone cement and preparation method thereof

Magnetic antibacterial bone cement is prepared by using 440C martensite silver powder and polymethyl methacrylate in bone cement, which solves the problem of insufficient anti-bone tumor and antibacterial properties of bone cement, and achieves moderate magnetothermal heating and high-temperature sterilization effect reduces the risk of damage to tissue by temperature.

CN118903548AActive Publication Date: 2024-11-08TIANJIN UNIV

Patent Information

Application Number
CN202411013956.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The existing bone cement lacks anti-bone tumor and antibacterial properties, which can easily lead to infection at the implanted site. The iron tetroxide warms up too quickly under the alternating magnetic field, which poses a risk of burning.

Method used

Magnetic antibacterial bone cement composed of 440C martensite silver powder and polymethyl methacrylate, and 440C martensite silver powder with large and particle size are prepared by alcohol slurry, flotation, filtration and adhesion, and vacuum drying. , replace Fe3O4 magnetic substances, control the magneto-heat heating rate, enhance development and antibacteriality, and form an electromagnetic shielding network structure.

Benefits of technology

Magnetic antibacterial bone cement with moderate magneto-heat heating rate is achieved, and long-term stable development can kill tumor cells, prolong the solidification time, reduce the risk of thermal damage, and enhance the wear resistance and durability of bone cement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118903548A_ABST
    Figure CN118903548A_ABST
Patent Text Reader

Abstract

The invention relates to magnetic antibacterial bone cement and a preparation method, the bone cement is composed of a powder part and a liquid part, the ratio of the powder part to the liquid part is (2-3): 1g / mL, and the powder part comprises the following components in percentage by mass: 45-89% of polymethyl methacrylate, 10-50% of 440C martensitic steel silver powder and 1-5% of benzoyl peroxide; in the 440C martensitic steel silver powder, the mass percentage content of the 440C martensitic stainless steel powder is 65-95%, and the mass percentage content of the silver powder is 5-35%; the liquid component comprises the following components in percentage by mass: 94.90 to 99.89 percent of methyl methacrylate monomer, 0.1 to 5 percent of N, N-dimethyl p-toluidine and 0.01 to 0.1 percent of hydroquinone. The bone cement disclosed by the invention is moderate in magnetic heating rate, can realize long-term stable development, and has certain antibacterial activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of bone repair materials, and particularly relates to a magnetic antibacterial bone cement and a preparation method thereof. Background Art

[0002] The relevant technologies of artificial joint replacement are becoming more and more mature, and the long-term survival rate of prostheses has been significantly improved compared with before. However, various reasons can lead to the failure of joint prostheses. At present, it is found in clinical practice that factors such as aseptic loosening and deep infection can lead to the failure of joint replacement. Bone tumors or bone metastasis of malignant tumors are also one of the reasons for the failure of joint prosthesis fixation. For bone tumors, surgical resection is often chosen, and other means such as chemotherapy and radiotherapy are used for postoperative treatment. With the current serious problems of atmospheric and water pollution, the prominent aging population, and the improvement of medical and health conditions, the life expectancy of patients with malignant tumors has been extended. It is expected that the number of cases of bone tumors will increase day by day. China has a large population base, and there will be more patients with bone metastases. Bone tumors or osteoarticular infections often cause bone defects. It is crucial to implant excellent filling materials to repair bone defects and reconstruct bone mechanical properties. Bone cement has excellent biocompatibility, plasticity and curing ability, and is widely used in clinical practice. However, bone cement lacks the function of anti-bone tumors and lacks antibacterial properties, which can easily lead to infection at the implantation site.

[0003] Many scholars have modified bone cement by loading drugs, doping particles with magnetocaloric or photothermal properties, etc. to give it anti-tumor function or bactericidal and antibacterial properties. The most commonly used magnetic materials are ferric oxide or ferric oxide magnetic powders. The team of Yuanyi Zheng and Zhechuan Mei successfully thermally removed liver tumors in animals by adding ferric oxide to PMMA bone cement and calcium phosphate bone cement. However, single ferric oxide has the problem of poor heat transfer efficiency in anti-tumor applications, and the heating rate of ferric oxide is too fast under an alternating magnetic field, and the extreme temperature can reach 500°C, which poses a risk of burning other tissues, and ferric oxide has no antibacterial properties. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a magnetic antibacterial bone cement having a moderate magnetic thermal heating rate, capable of achieving long-term stable development and having certain antibacterial properties, and a preparation method thereof.

[0005] One of the above objects of the present invention is achieved by the following technical solution:

[0006] A magnetic antibacterial bone cement, composed of two parts, powder and liquid, the ratio of powder to liquid is (2-3): 1g / mL,

[0007] The powder components and mass percentages are: 45-89% of polymethyl methacrylate, 10-50% of 440C martensitic steel silver powder, and 1-5% of benzoyl peroxide; in the 440C martensitic steel silver powder, the mass percentage of 440C martensitic stainless steel powder is 65-95%, and the mass percentage of silver powder is 5-35%;

[0008] The liquid components and their mass percentages are: 94.90-99.89% of methyl methacrylate monomer, 0.1-5% of N,N-dimethyl-p-toluidine, and 0.01-0.1% of hydroquinone.

[0009] Furthermore, the particle size distribution range of polymethyl methacrylate is 0.2 to 150 μm, and the molecular weight is 100,000 to 1,000,000.

[0010] Moreover, the particle size distribution range of 440C martensitic steel silver powder is 0.1 to 100 μm.

[0011] Moreover, the particle size distribution range of the 440C martensitic steel powder in the 440C martensitic steel silver powder is 2.6 to 100 μm, and the particle size distribution range of the silver powder is 0.1 to 45 μm.

[0012] Moreover, the preparation method of 440C martensitic steel silver powder is:

[0013] (1) putting 440C martensitic steel powder into anhydrous ethanol, with the ratio of steel powder to anhydrous ethanol being (1:5) to 10, and stirring continuously for 10 to 60 minutes to obtain a steel powder ethanol mixed slurry;

[0014] (2) adding silver powder into anhydrous ethanol, wherein the ratio of silver powder to anhydrous ethanol is (1:5) to 20, and stirring is continued for 10 to 60 minutes to obtain a silver powder ethanol mixed slurry;

[0015] (3) adding the mixed slurry of step (2) to the steel powder ethanol mixed slurry of step (1) and mixing for 10 to 30 minutes;

[0016] (4) After mixing evenly, sieving and filtering to remove excess anhydrous ethanol to obtain wet 440C martensitic steel silver powder;

[0017] (5) The composite powder is then transferred to a vacuum oven, the vacuum degree is maintained at less than 5 Pa, and dried at 37-100° C. for 3-24 h;

[0018] (6) The dried and cooled composite powder is ball-milled for 1 to 3 hours and sieved to obtain the desired 440C martensitic steel silver powder.

[0019] The second objective of the present invention is achieved by the following technical solutions:

[0020] A method for preparing the above-mentioned magnetic antibacterial bone cement comprises the following steps:

[0021] (1) polymethyl methacrylate, benzoyl peroxide and 440C martensitic steel silver powder are uniformly mixed in a mixing device for 3 to 24 hours;

[0022] (2) The uniformly mixed bone cement powder is taken out, and the powder and liquid are weighed separately according to the ratio of bone cement powder to liquid of (2-3):1 g / mL, and the bone cement liquid is added to the bone cement powder and stirred for 10-60 seconds to prepare bone cement.

[0023] The advantages and positive effects of the present invention are:

[0024] The present invention selects 440C martensitic steel powder (micron particles) and silver powder (including nanoparticles) with different particle size distribution ranges, and obtains 440C martensitic steel silver powder with large and small particle size distribution through alcohol slurry, flotation, filtration attachment, and vacuum drying. The obtained 440C martensitic steel silver powder is then added to bone cement, and the developer and Fe3O4 magnetic material in the bone cement are replaced at the same time, which can prevent the conventional Fe3O4 magnetic material from heating up too fast under an alternating magnetic field, and the risk of burning other tissues due to excessive temperature, and give the bone cement a certain developing property, with the advantages of moderate magnetic thermal heating rate and long-term stable development. At the same time, the wear resistance and durability of the bone cement are enhanced. The 440C martensitic steel silver powder in the bone cement can kill or eliminate tumor cells by heating the bone cement to a temperature of more than 40°C through an alternating magnetic field and hysteresis, and has the effect of high temperature sterilization, and prolongs the solidification time of the bone cement, prevents the rapid accumulation of energy in the polymerization process, and reduces the thermal damage of the bone cement polymerization to the tissue. At the same time, the unique antibacterial property of silver can enhance the antibacterial property of bone cement. At the same time, the 440C martensitic steel silver powder is evenly distributed in the bone cement to form an electromagnetic shielding network structure. The reflected part of the electromagnetic wave plays an electromagnetic shielding effect, which can reduce the maximum temperature of the hysteresis heating of the bone cement and prevent the thermal damage of the tissue to the magnetocaloric effect. The prepared magnetic antibacterial bone cement has the characteristics of injectability and appropriate strength, and can be used for the fixation of various fractures and the filling of bone defects. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is the development picture of the magnetic antibacterial bone cement tested in Examples 1-3 of the present invention and the existing control joint cement, and the second column in the figure is not used in the present invention;

[0026] Figure 2 These are pictures of the temperature rise results of testing magnetic antibacterial bone cement under a magnetic field in Examples 1-3 of the present invention, 2a, control sample, 2b, sample of Example 1, 2c, sample of Example 2, 2d, sample of Example 3. DETAILED DESCRIPTION

[0027] The structure of the present invention is further described below with reference to the accompanying drawings and by way of examples. It should be noted that the present examples are descriptive rather than restrictive.

[0028] A magnetic antibacterial bone cement, composed of two parts, powder and liquid, the ratio of powder to liquid is (2-3): 1g / mL,

[0029] The powder components and mass percentages are: 45-89% polymethyl methacrylate, 10-50% 440C martensitic steel silver powder, and 1-5% benzoyl peroxide. Among them, the mass percentage of 440C martensitic steel silver powder is preferably 10-42%; further, the mass percentage of 440C martensitic steel silver powder is preferably 10-30%. In the 440C martensitic steel silver powder, the mass percentage of 440C martensitic stainless steel powder is 65-95%, and the mass percentage of silver powder is 5-35%. Further, in the 440C martensitic steel silver powder, the mass percentage of 440C martensitic stainless steel powder is 74-92%, and the mass percentage of silver is 8-26%.

[0030] The liquid components and their mass percentages are: 94.90-99.89% of methyl methacrylate monomer, 0.1-5% of N,N-dimethyl-p-toluidine, and 0.01-0.1% of hydroquinone.

[0031] The particle size distribution range of the polymethyl methacrylate is 0.2 to 150 μm, and the molecular weight is 100,000 to 1,000,000. The particle size distribution range of the polymethyl methacrylate powder is preferably 5 to 80 μm, and the molecular weight range is preferably 200,000 to 600,000. Furthermore, the particle size distribution range of the polymethyl methacrylate powder is preferably 20 to 60 μm, and the molecular weight range is preferably 300,000 to 500,000.

[0032] The particle size distribution range of the above 440C martensitic steel silver powder is 0.1-100 μm. The particle size distribution range of the 440C martensitic steel silver powder is preferably 0.3-74 μm; further, the particle size distribution range of the 440C martensitic steel silver powder is preferably 0.45-45 μm.

[0033] The particle size distribution range of the 440C martensitic steel powder in the above 440C martensitic steel silver powder is 2.6-100 μm, and the particle size distribution range of the silver powder is 0.1-45 μm.

[0034] The preparation method of the above 440C martensitic steel silver powder is as follows:

[0035] (1) putting 440C martensitic steel powder into anhydrous ethanol, with the ratio of steel powder to anhydrous ethanol being (1:5) to 10, and stirring continuously for 10 to 60 minutes to obtain a steel powder ethanol mixed slurry;

[0036] (2) adding silver powder into anhydrous ethanol, wherein the ratio of silver powder to anhydrous ethanol is (1:5) to 20, and stirring is continued for 10 to 60 minutes to obtain a silver powder ethanol mixed slurry;

[0037] (3) adding the mixed slurry of step (2) to the steel powder ethanol mixed slurry of step (1) and mixing for 10 to 30 minutes;

[0038] (4) After mixing evenly, sieving and filtering to remove excess anhydrous ethanol to obtain wet 440C martensitic steel silver powder;

[0039] (5) The composite powder is then transferred to a vacuum oven, the vacuum degree is maintained at less than 5 Pa, and dried at 37-100° C. for 3-24 h;

[0040] (6) The dried and cooled composite powder is ball-milled for 1 to 3 hours and sieved to obtain the desired 440C martensitic steel silver powder.

[0041] The preparation method of the magnetic antibacterial bone cement of the present invention comprises the following steps:

[0042] (1) polymethyl methacrylate, benzoyl peroxide and 440C martensitic steel silver powder are uniformly mixed in a mixing device for a mixing time of 3 to 24 hours;

[0043] (2) The uniformly mixed bone cement powder is taken out, and the powder and liquid are weighed separately according to the ratio of bone cement powder to liquid of (2-3):1 g / mL, and the bone cement liquid is added to the bone cement powder and stirred for 10-60 seconds to prepare bone cement.

[0044] Example 1

[0045] A magnetic antibacterial bone cement comprises powder and liquid, wherein the ratio of the powder to the liquid is 2.5:1 (g / mL); the powder comprises: 68% of polymethyl methacrylate, 30% of 440C martensitic steel silver powder, and 2% of benzoyl peroxide; the liquid comprises: 98.9% of methyl methacrylate monomer, 1% of N,N-dimethyl-p-toluidine and 0.1% of hydroquinone; the particle size distribution range of the polymethyl methacrylate is 0.2-150 μm, and the molecular weight is 350,000; the particle size distribution range of the 440C martensitic steel silver powder is 0.3-74 μm; in the 440C martensitic steel silver powder, the mass percentage content of 440C martensitic stainless steel powder is 92%, and the mass percentage content of silver is 8%.

[0046] The pretreatment method of 440C martensitic steel silver powder is:

[0047] (1) Put 440C martensitic steel powder into anhydrous ethanol, the ratio of steel powder to anhydrous ethanol is 1:10, and stir for 60 minutes to obtain a steel powder ethanol mixed slurry;

[0048] (2) adding silver powder to anhydrous ethanol in a ratio of 1:20, and stirring for 60 minutes to obtain a silver powder ethanol mixed slurry;

[0049] (3) adding the mixed slurry of step (2) to the steel powder ethanol mixed slurry of step (1) and mixing for 30 minutes;

[0050] (4) After mixing evenly, sieving and filtering to remove excess anhydrous ethanol to obtain wet 440C martensitic steel silver powder;

[0051] (5) The composite powder is then transferred to a vacuum oven, the vacuum degree is maintained at less than 5 Pa, and dried at 100 ° C for 3 h;

[0052] (6) ball milling the dried and cooled composite powder for 3 h and screening to obtain the desired 440C martensitic steel silver powder;

[0053] The preparation method of magnetic antibacterial bone cement is as follows:

[0054] (1) polymethyl methacrylate, benzoyl peroxide and 440C martensitic steel silver powder were mixed uniformly in a mixing device for 3 hours;

[0055] (2) Take out the evenly mixed bone cement powder, weigh the powder and liquid according to the ratio of bone cement powder to liquid of 2.5:1 (g / mL), add the bone cement liquid to the bone cement powder, stir for 30 seconds, and complete the preparation of bone cement.

[0056] The prepared bone cement is filled into the fracture or bone defect site that needs to be filled or stabilized. It can be operated for 17 minutes and solidified in 28 minutes.

[0057] The prepared bone cement was used to make disc samples with a diameter of 3 mm and a thickness of 3 mm. The samples were photographed and observed under X-ray and compared with the conventional joint bone cement samples. Figure 1 As shown, the sample of Example 1 is also clearly visible under X-ray, indicating that the magnetic antibacterial bone cement of the present invention has good developing properties.

[0058] The bone cement sample of Example 1 was tested in an alternating magnetic field. The temperature of the bone cement could reach 64.3°C within 2 minutes under an alternating magnetic field of 50KHz, which was lower than 81.2°C of the control sample (iron tetroxide-containing bone cement). This indicates that the temperature rise of the magnetic antibacterial bone cement of the present invention is lower than that of the existing bone cement under a variable magnetic field, thereby avoiding the risk of overheating and burning other tissues during use.

[0059] Example 2

[0060] A magnetic antibacterial bone cement comprises powder and liquid, wherein the ratio of the powder to the liquid is 2:1 (g / mL); the powder comprises: 77% of polymethyl methacrylate, 20% of 440C martensitic steel silver powder, and 3% of benzoyl peroxide; the liquid comprises: 96.9% of methyl methacrylate monomer, 3% of N,N-dimethyl-p-toluidine and 0.1% of hydroquinone; the particle size distribution range of the polymethyl methacrylate is 5-80 μm, and the molecular weight is 350,000; the particle size distribution range of the 440C martensitic steel silver powder is 0.45-45 μm; in the 440C martensitic steel silver powder, the mass percentage content of 440C martensitic stainless steel powder is 74%, and the mass percentage content of silver is 26%.

[0061] The pretreatment method of 440C martensitic steel silver powder is:

[0062] (1) Put 440C martensitic steel powder into anhydrous ethanol, the ratio of steel powder to anhydrous ethanol is 1:8, and stir for 10 minutes to obtain a steel powder ethanol mixed slurry;

[0063] (2) adding silver powder to anhydrous ethanol in a ratio of 1:15, and stirring for 30 minutes to obtain a silver powder ethanol mixed slurry;

[0064] (3) adding the mixed slurry of step (2) to the steel powder ethanol mixed slurry of step (1) and mixing for 10 minutes;

[0065] (4) After mixing evenly, sieving and filtering to remove excess anhydrous ethanol to obtain wet 440C martensitic steel silver powder;

[0066] (5) The composite powder is then transferred to a vacuum oven, the vacuum degree is maintained at less than 5 Pa, and dried at 70 ° C for 5 h;

[0067] (6) ball milling the dried and cooled composite powder for 2 h and screening to obtain the desired 440C martensitic steel silver powder;

[0068] The preparation method of magnetic antibacterial bone cement is as follows:

[0069] (1) polymethyl methacrylate, benzoyl peroxide and 440C martensitic steel silver powder were mixed uniformly in a mixing device for 3 hours;

[0070] (2) Take out the evenly mixed bone cement powder, weigh the powder and liquid separately according to the ratio of bone cement powder to liquid of 2:1 (g / mL), add the bone cement liquid to the bone cement powder, stir for 30 seconds, and complete the preparation of bone cement.

[0071] The prepared bone cement was filled into the fracture or bone defect site to be filled or stabilized. The operation time was 14 minutes and the curing was completed in 23 minutes.

[0072] The bone cement prepared in Example 2 was made into a disc sample with a diameter of 3 mm and a thickness of 3 mm, and photographed and observed under X-ray, and compared with the conventional joint bone cement sample. Figure 1 As shown, the sample of Example 2 is also clearly visible under X-ray, indicating that the magnetic antibacterial bone cement of the present invention has good developing properties.

[0073] The bone cement sample of Example 2 was tested in an alternating magnetic field. The temperature of the bone cement could reach 55.5°C within 2 minutes under an alternating magnetic field of 50KHz, which was lower than 81.2°C of the control sample (iron tetroxide-containing bone cement). This indicates that the temperature rise of the magnetic antibacterial bone cement of the present invention is lower than that of the existing bone cement under a variable magnetic field, thereby avoiding the risk of overheating and burning other tissues during use.

[0074] Example 3

[0075] A magnetic antibacterial bone cement comprises powder and liquid, wherein the ratio of the powder to the liquid is 2:1 (g / mL); the powder comprises: 85% of polymethyl methacrylate, 10% of 440C martensitic steel silver powder, and 5% of benzoyl peroxide; the liquid comprises: 94.99% of methyl methacrylate monomer, 5% of N,N-dimethyl-p-toluidine and 0.01% of hydroquinone; the particle size distribution range of the polymethyl methacrylate is 5-80 μm, and the molecular weight is 350,000; the particle size distribution range of the 440C martensitic steel silver powder is 0.45-45 μm; in the 440C martensitic steel silver powder, the mass percentage of 440C martensitic stainless steel powder is 65%, and the mass percentage of silver is 35%.

[0076] The pretreatment method of 440C martensitic steel silver powder is:

[0077] (1) Put 440C martensitic steel powder into anhydrous ethanol, with the ratio of steel powder to anhydrous ethanol being 1:5, and stir for 20 minutes to obtain a steel powder ethanol mixed slurry;

[0078] (2) adding silver powder to anhydrous ethanol in a ratio of 1:16, and stirring for 20 minutes to obtain a silver powder ethanol mixed slurry;

[0079] (3) adding the mixed slurry from step (2) to the steel powder ethanol mixed slurry from step (1) and mixing for 20 minutes;

[0080] (4) After mixing evenly, sieving and filtering to remove excess anhydrous ethanol to obtain wet 440C martensitic steel silver powder;

[0081] (5) The composite powder is then transferred to a vacuum oven, the vacuum degree is maintained at less than 5 Pa, and dried at 80 ° C for 4 h;

[0082] (6) ball-milling the dried and cooled composite powder for 1 h and screening to obtain the desired 440C martensitic steel silver powder;

[0083] The preparation method of magnetic antibacterial bone cement is as follows:

[0084] (1) polymethyl methacrylate, benzoyl peroxide and 440C martensitic steel silver powder were mixed uniformly in a mixing device for 3 hours;

[0085] (2) Take out the evenly mixed bone cement powder, weigh the powder and liquid separately according to the ratio of bone cement powder to liquid of 2:1 (g / mL), add the bone cement liquid to the bone cement powder, stir for 30 seconds, and complete the preparation of bone cement.

[0086] The prepared bone cement is filled into the fracture or bone defect site that needs to be filled or stabilized. The operation time is 8 minutes and the curing is completed in 15 minutes.

[0087] The bone cement prepared in Example 3 was made into a disc sample with a diameter of 3 mm and a thickness of 3 mm, and photographed and observed under X-ray, and compared with the conventional joint bone cement sample. Figure 1 As shown, the sample of Example 3 is also clearly visible under X-ray. This shows that the magnetic antibacterial bone cement of the present invention has good developing properties.

[0088] The bone cement sample of Example 3 was tested in an alternating magnetic field. The temperature of the bone cement could reach 41.8°C within 2 minutes under an alternating magnetic field of 50KHz, which was lower than 81.2°C of the control sample (iron tetroxide-containing bone cement). This indicates that the temperature rise of the magnetic antibacterial bone cement of the present invention is lower than that of the existing bone cement under a variable magnetic field, thereby avoiding the risk of overheating and burning other tissues during use.

[0089] Example 4

[0090] A magnetic antibacterial bone cement comprises powder and liquid, wherein the ratio of the powder to the liquid is 2:1 (g / mL); the powder comprises: 53% of polymethyl methacrylate, 42% of 440C martensitic steel silver powder, and 5% of benzoyl peroxide; the liquid comprises: 94.99% of methyl methacrylate monomer, 5% of N,N-dimethyl-p-toluidine and 0.01% of hydroquinone; the particle size distribution range of the polymethyl methacrylate is 10-80 μm, and the molecular weight is 350,000; the particle size distribution range of the 440C martensitic steel silver powder is 15-53 μm; in the 440C martensitic steel silver powder, the mass percentage content of 440C martensitic stainless steel powder is 95%, and the mass percentage content of silver is 5%.

[0091] The pretreatment method of 440C martensitic steel silver powder is:

[0092] (1) Put 440C martensitic steel powder into anhydrous ethanol, with the ratio of steel powder to anhydrous ethanol being 1:5, and stir for 20 minutes to obtain a steel powder ethanol mixed slurry;

[0093] (2) adding silver powder to anhydrous ethanol in a ratio of 1:13, and stirring for 20 min to obtain a silver powder ethanol mixed slurry;

[0094] (3) adding the mixed slurry from step (2) to the steel powder ethanol mixed slurry from step (1) and mixing for 20 minutes;

[0095] (4) After mixing evenly, sieving and filtering to remove excess anhydrous ethanol to obtain wet 440C martensitic steel silver powder;

[0096] (5) The composite powder is then transferred to a vacuum oven, the vacuum degree is maintained at less than 5 Pa, and dried at 80 ° C for 4 h;

[0097] (6) ball-milling the dried and cooled composite powder for 1 h and screening to obtain the desired 440C martensitic steel silver powder;

[0098] The preparation method of magnetic antibacterial bone cement is as follows:

[0099] (1) polymethyl methacrylate, benzoyl peroxide and 440C martensitic steel silver powder were uniformly mixed in a mixing device for 3 hours;

[0100] (2) Take out the evenly mixed bone cement powder, weigh the powder and liquid separately according to the ratio of bone cement powder to liquid of 2:1 (g / mL), add the bone cement liquid to the bone cement powder, stir for 30 seconds, and complete the preparation of bone cement.

[0101] The prepared bone cement is filled into the fracture or bone defect site that needs to be filled or stabilized. The operation time is 18 minutes and the curing is completed in 30 minutes.

[0102] Test Example 1

[0103] The physical properties of the bone cements prepared in Examples 1-4 were tested, and the test results are shown in Table 1:

[0104] Table 1

[0105] Test No. Compression strength(MPa) Flexural strength(MPa) Flexural modulus (MPa) Example 1 92.92±1.81 74.93±7.86 3369.28±231.05 Example 2 92.94±3.78 73.24±4.75 3564.29±232.60 Example 3 92.60±5.15 71.73±4.40 3427.19±179.07 Example 4 90.50±3.78 62.66±2.23 3046.41±175.64

[0106] It can be seen from Table 1 that the mechanical properties of the magnetic antibacterial bone cement in Examples 1-4 of the present invention after curing meet the requirements of the bone cement industry standard YY0459.

[0107] In the present invention, 440C martensitic steel powder is prepared from conventional 440C stainless steel. 440C martensitic steel powder is commonly used in high-hardness cutting tools, abrasive tools, and 3D printing, and has good hardness, wear resistance, and corrosion resistance. The silver powder has good antibacterial properties. The electromagnetic shielding network structure formed by 440C martensitic steel silver powder in bone cement reflects part of the electromagnetic waves to play an electromagnetic shielding effect, which can reduce the maximum temperature of bone cement magnetocaloric effect and prevent thermal damage to tissues by magnetocaloric effect. The bone cement of the present invention is mainly used for filling or stabilizing fracture sites or bone defect sites.

[0108] The above-mentioned specific implementations are only specific cases of the present invention. The patent protection scope of the present invention includes but is not limited to the product form and style of the above-mentioned specific implementations. Any appropriate changes or modifications made to them by ordinary technicians in the technical field that conform to the claims of the present invention shall fall within the patent protection scope of the present invention.

Claims

1. A magnetic antibacterial bone cement, Features: It consists of two parts: powder and liquid, with the ratio of powder to liquid being (2-3):1g / mL; The powder components and mass percentages are: 45-89% of polymethyl methacrylate, 10-50% of 440C martensitic steel silver powder, and 1-5% of benzoyl peroxide; in the 440C martensitic steel silver powder, the mass percentage of 440C martensitic stainless steel powder is 65-95%, and the mass percentage of silver powder is 5-35%; The liquid components and their mass percentages are: 94.90-99.89% of methyl methacrylate monomer, 0.1-5% of N,N-dimethyl-p-toluidine, and 0.01-0.1% of hydroquinone.

2. The magnetic antibacterial bone cement according to claim 1, Features: The particle size distribution range of polymethyl methacrylate is 0.2 to 150 μm, and the molecular weight is 100,000 to 1,000,000.

3. The magnetic antibacterial bone cement according to claim 1, Features: The particle size distribution range of 440C martensitic steel silver powder is 0.1 to 100 μm.

4. The magnetic antibacterial bone cement according to claim 1, Features: The particle size distribution range of the 440C martensitic steel powder in the 440C martensitic steel silver powder is 2.6-100 μm, and the particle size distribution range of the silver powder is 0.1-45 μm.

5. The magnetic antibacterial bone cement according to claim 1, Features: The preparation method of 440C martensitic steel silver powder is: (1) putting 440C martensitic steel powder into anhydrous ethanol, with the ratio of steel powder to anhydrous ethanol being (1:5) to 10, and stirring continuously for 10 to 60 minutes to obtain a steel powder ethanol mixed slurry; (2) adding silver powder into anhydrous ethanol, wherein the ratio of silver powder to anhydrous ethanol is (1:5) to 20, and stirring is continued for 10 to 60 minutes to obtain a silver powder ethanol mixed slurry; (3) adding the mixed slurry of step (2) to the steel powder ethanol mixed slurry of step (1) and mixing for 10 to 30 minutes; (4) After mixing evenly, sieving and filtering to remove excess anhydrous ethanol to obtain wet 440C martensitic steel silver powder; (5) The composite powder is then transferred to a vacuum oven, the vacuum degree is maintained at less than 5 Pa, and dried at 37-100° C. for 3-24 h; (6) The dried and cooled composite powder is ball-milled for 1 to 3 hours and sieved to obtain the desired 440C martensitic steel silver powder.

6. A method for preparing the magnetic antibacterial bone cement as claimed in any one of claims 1 to 5, comprising the following steps: (1) polymethyl methacrylate, benzoyl peroxide and 440C martensitic steel silver powder are uniformly mixed in a mixing device for a mixing time of 3 to 24 hours; (2) The uniformly mixed bone cement powder is taken out, and the powder and liquid are weighed separately according to the ratio of bone cement powder to liquid of (2-3):1 g / mL, and the bone cement liquid is added to the bone cement powder and stirred for 10-60 seconds to prepare bone cement.

Citation Information

Patent Citations

  • Bone cement having antibiosis and biological compatibility and preparation method thereof

    CN107625993A

  • Magnetic bioglass bone cement and preparation method thereof

    CN112206346A

  • Antibacterial bone cement and preparation method thereof

    CN113876998A

  • Production of magnetic powder for electromagnetic connecting device

    JP1995216403A

  • Chromium-nickel steel, martensitic wire and method for production thereof

    US20150027598A1

Cited By

  • Photo-thermal controlled release H2S polyurethane reinforced bone cement and preparation method thereof

    CN120459369A