Separation equipment based on vacuum distillation and method for vacuum separation and purification of indium-tin lead-free solder

Through vacuum distillation combined with condenser directional condensation technology, the existing indium tin alloy separation methods have solved the problems of high energy consumption and low purity, and the efficient separation and purification of indium tin is achieved. It is suitable for indium tin alloys with low indium content, which has improved the Product purity and process efficiency.

CN118910436APending Publication Date: 2024-11-08KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410969294.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing indium tin alloy separation method consumes high energy, consumes a lot of reagents, has a lot of waste, and has low recovery rate. It cannot effectively improve the indium and tin purity of the product. Especially when treating indium tin alloys with low indium content, the application of traditional processes is applicable. Insufficient in nature and purity.

Method used

Using a separation equipment based on vacuum distillation, combined with the condenser design, the efficient separation of indium tin is achieved through the crucible and condenser in the vacuum distillation furnace. Using the directional condensation technology of the condensation disk and the condensation cover, indium vapor condenses on the condensation cover, and tin is used. Condensation in a condensation dish, efficient separation and purification of indium and tin is achieved through an evaporation-directional condensation cycle.

Benefits of technology

The purity of indium and tin is improved, with indium content ≥93% and tin content ≥84%. It is suitable for indium tin alloys with low indium content, reducing metal losses and improving the efficiency and purity of the separation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910436A_ABST
    Figure CN118910436A_ABST
Patent Text Reader

Abstract

The invention provides separation equipment based on vacuum distillation and a method for vacuum separation and purification of indium-tin lead-free solder, and belongs to the technical field of alloy separation and purification. The separation equipment based on vacuum distillation comprises a vacuum distillation furnace, the vacuum distillation furnace comprises a crucible, and the crucible is used for containing materials to be separated; the open end of the crucible is connected with a condenser, and the condenser comprises a condensing disc and a condensing cover; a through hole is formed in the center of the bottom of the condensing disc to serve as a steam channel. A cofferdam is arranged around the through hole; the inner surface of the condensation cover is an arc-shaped curved surface and is sunken upwards; and the condensing disc and the condensing cover are in sealing fit. According to the invention, vacuum distillation and condensation are combined, indium generated during heating together with mixed steam of a small amount of tin volatilizes out of the crucible and enters the condensation disc, most of tin remains in the crucible, tin in the mixed steam is condensed in the condensation disc, indium is condensed to the condensation cover, and efficient separation and purification of indium and tin are realized through vacuum evaporation-directional condensation circulation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of separation and purification of alloys, and in particular relates to separation equipment based on vacuum distillation and a method for vacuum separation and purification of indium tin lead-free solder. Background Art

[0002] Indium tin lead-free solder has the advantages of low melting point, low tensile strength, good thermal fatigue resistance, good conductivity, and reliable connection performance. It is often used for the connection of electronic components, such as welding on circuit boards and packaging of semiconductor devices. It has become one of the main special solders for tiny packages and high-density electronic devices. With the rapid development of global science and technology, electronic products are rapidly upgraded and replaced, and the scrapping of electronic products has become a trend. As one of the solders in discarded electronic products, the comprehensive recycling of indium tin lead-free solder is of great significance.

[0003] At present, the separation method of indium tin alloy is to perform wet or fire separation on the recycled ITO waste targets (the In content in the ITO target is 90-95%, and the Sn content is 5-10%) or crude indium (In content ≥90%). The wet method is the first choice for recycling ITO waste targets. First, the indium tin oxide in the waste targets is separated in an acidic solution, and then In and Sn are separated by solvent extraction, resin separation or sulfide precipitation. This method consumes a lot of reagents, the process is complicated and lengthy, and a large amount of waste is generated. The pyrometallurgical method includes evaporation, chlorination, vacuum carbon thermal reduction and other methods. The evaporation method utilizes the different saturated vapor pressures of In2O3 and SnO2. At a high temperature above 2273K, indium tin oxide in the waste target is recovered by DC arc or plasma evaporation, which has high energy consumption. The chlorination method is to reduce ITO to InCl3 for recycling. It has the advantages of short process flow and less time consumption, but the recovery rate is low and no elemental metal can be obtained. The vacuum carbon thermal reduction method reduces ITO at 1223K by adding 30wt% of carbon. The reduction rate is as high as 90%, but the carbon consumption is large, and the purity of the product indium and tin is low. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a separation device based on vacuum distillation and a method for vacuum separation and purification of indium tin lead-free solder. The condensation device provided by the present invention can achieve separation and purification of indium tin lead-free solder and improve the purity of product indium and tin.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] The present invention provides a separation device based on vacuum distillation, comprising a vacuum distillation furnace, wherein the vacuum distillation furnace comprises a crucible for containing materials to be separated; an open end of the crucible is connected to a condenser, and the condenser comprises a condensation plate and a condensation cover;

[0007] A through hole is provided at the center of the bottom of the condensation plate as a steam passage; and a cofferdam is provided around the through hole;

[0008] The inner surface of the condensation cover is an arc-shaped curved surface, which is concave upwards;

[0009] The condensation tray and the condensation cover are sealed together.

[0010] Preferably, the diameter of the through hole is 40-50 mm.

[0011] Preferably, the height of the cofferdam is 8-15 mm.

[0012] Preferably, the condensation tray has a depth of 45 to 55 mm and an inner diameter of 160 to 200 mm.

[0013] Preferably, the inner surface of the condensation tray is an arc-shaped surface with a curvature radius of 25 to 35 mm.

[0014] Preferably, the maximum vertical distance between the condensation cover and the condensation tray is 50-60 mm.

[0015] Preferably, the depth of the graphite crucible in the vacuum distillation furnace is 110-140 mm.

[0016] The present invention also provides a method for vacuum separation and purification of indium tin lead-free solder, using the separation equipment described in the above technical solution, comprising the following steps:

[0017] Placing the indium tin lead-free solder in the crucible of the separation device for vacuum distillation to obtain a residue and volatile vapor;

[0018] The volatile vapor passes through the through holes of the condensation tray and is condensed in the condenser, thereby obtaining a metal indium product in the condensation tray and the condensation cover, and obtaining a residual metal tin product in the crucible.

[0019] Preferably, the temperature during the vacuum distillation is 1100-1300°C;

[0020] The vacuum distillation time is 400 to 480 minutes;

[0021] The pressure of the vacuum distillation is 0.1-1Pa.

[0022] Preferably, the mass percentage of indium in the indium-tin lead-free solder is 48-55%, and the mass percentage of tin is 45-52%.

[0023] The present invention provides a separation device based on vacuum distillation, including a vacuum distillation furnace, wherein the vacuum distillation furnace includes a crucible for containing materials to be separated; the open end of the crucible is connected to a condenser, and the condenser includes a condensation tray and a condensation cover; a through hole is provided at the central position of the bottom of the condensation tray as a vapor passage; a cofferdam is provided around the through hole; the inner surface of the condensation cover is an arc-shaped curved surface, which is concave upward; and the condensation tray and the condensation cover are sealed. The present invention combines vacuum distillation with condensation, and a condenser is provided above the crucible, and a through hole is provided at the central position of the bottom of the condensation tray. During heating, the mixed vapor of indium and a small amount of tin produced by vacuum distillation evaporates from the crucible and enters the condensation tray, and most of the tin remains in the crucible. The condensation temperature of tin is high and it is preferentially condensed in the condensation tray. The indium vapor continues to rise and condenses onto the condensation cover. Through this directional condensation method, efficient separation and purification of indium and tin is achieved; a cofferdam is provided around the through hole to prevent the volatilized indium from flowing back into the crucible; the inner surface of the condensation cover is provided with a cofferdam. The arc-shaped surface is concave upward. During the condensation process of the mixed vapor, the liquid condensate will gather in the middle of the condensation cover. When it accumulates to a certain extent, it will drip into the graphite crucible and then undergo an evaporation-directional condensation cycle. Due to the presence of the through hole, the middle of the condensation cover is radiated by the heat source of the lower heating element, resulting in a higher middle temperature than the surrounding temperature, so that tin is mainly gathered in the middle of the condensation cover, and indium is mainly condensed around the condensation cover, thereby achieving separation of indium and tin. The condensation plate and the condensation cover are sealed to achieve a closed cycle without metal loss, thereby improving the direct recovery rate of indium.

[0024] The present invention also provides a method for vacuum separation and purification of indium tin lead-free solder, which combines the vacuum distillation theory with the condensation theory to achieve efficient separation and purification of indium and tin in one step, thereby improving the purity of the product indium and tin. The test results show that the vacuum separation and purification method of indium tin lead-free solder implemented by the present invention using a condensation device has an indium content of ≥93% on the condensation cover and the condensation plate, and a tin content of ≥84% in the graphite crucible.

[0025] In addition, the raw materials for the current indium tin alloy processing process are mainly ITO waste target materials and crude indium, and the indium content is more than 90%, which indirectly indicates that the traditional vacuum processing process can only process indium tin alloy waste with a very high indium content, but the method and separation equipment of the present invention can process indium tin alloy with an indium content as low as 52%, with stronger applicability and higher product purity. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0027] Figure 1 A structural schematic diagram and a condensation principle diagram of the separation device used in the present invention;

[0028] Figure 2 A side view of a condensation tray in a condensation device used in Examples 1 to 5 and Comparative Examples 1 to 3;

[0029] Figure 3 A top view of a condensation plate in a condensation device used in Examples 1 to 5 and Comparative Examples 1 to 3;

[0030] Figure 4 A side view of a condensation cover in a condensation device used in Examples 1 to 5 and Comparative Examples 1 to 3;

[0031] Figure 5 It is a top view of the condensation cover in the condensation device used in Examples 1 to 5 and Comparative Examples 1 to 3. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The present invention provides a separation device based on vacuum distillation, comprising a vacuum distillation furnace, wherein the vacuum distillation furnace comprises a crucible for containing materials to be separated; an open end of the crucible is connected to a condenser, and the condenser comprises a condensation plate and a condensation cover;

[0034] A through hole is provided at the center of the bottom of the condensation plate as a steam passage; and a cofferdam is provided around the through hole;

[0035] The inner surface of the condensation cover is an arc-shaped curved surface, which is concave upwards;

[0036] The condensation tray and the condensation cover are sealed together.

[0037] like Figure 1 As shown, the separation equipment provided by the present invention includes a vacuum distillation furnace, and the vacuum distillation furnace includes a crucible. The crucible is surrounded by a heating element, and the heating element is wrapped with thermal insulation felt. The crucible is used to hold the material to be separated, the heating element provides high temperature, and the thermal insulation felt maintains the temperature in the vacuum distillation furnace to reduce energy consumption. The present invention has no special limitation on the material of the crucible, and a crucible well known in the art can be selected. A graphite crucible is used in a specific embodiment of the present invention. In the present invention, the depth of the crucible is preferably 110 to 140 mm, and more preferably 120 mm.

[0038] The separation device provided by the present invention comprises a condenser connected to the open end of the crucible, wherein the condenser comprises a condensation tray and a condensation cover. Figure 2 and Figure 3 As shown, a through hole is provided at the center of the bottom of the condensation tray as a vapor passage; and a cofferdam is provided around the through hole. During the vacuum distillation process, the material in the crucible is vaporized, and the obtained vapor passes through the opening of the crucible and enters the condenser from the through hole provided at the bottom of the condensation tray. The condensation tray is located above the crucible and the insulation felt, and its temperature is lower than that of the crucible. When the indium-tin alloy mixed vapor evaporates from the crucible, the tin with a higher condensation temperature condenses in the condensation tray, while the indium vapor continues to rise. The condensed liquid will gather in the condensation tray, and the presence of the cofferdam prevents the liquid from flowing back into the crucible.

[0039] In the present invention, the thickness of the condensation tray is preferably 8-15 mm, more preferably 10 mm; the diameter of the through hole is preferably 40-50 mm, more preferably 44 mm; the height of the cofferdam is preferably 8-15 mm, more preferably 10 mm; the thickness of the cofferdam is preferably 5-10 mm, more preferably 8 mm; the depth of the condensation tray is preferably 45-55 mm, more preferably 50 mm; the inner diameter of the condensation tray is preferably 160-200 mm, more preferably 180 mm. The inner surface of the condensation tray is an arc-shaped surface, and the radius of curvature is preferably 25-35 mm, more preferably 30 mm.

[0040] The inner surface of the condensation cover in the separation device provided by the present invention is an arc-shaped curved surface, which is concave upward. Specifically, the overall structure of the condensation cover is thin in the center and thick around. In the present invention, the difference between the center thickness and the surrounding thickness of the condensation cover is preferably 4-6 mm, more preferably 5 mm. In the present invention, the maximum vertical distance between the condensation cover and the condensation plate is preferably 50-60 mm, more preferably 55 mm. The inner surface of the condensation cover is an arc-shaped curved surface. After the indium vapor contacts the condensation cover whose temperature is lower than the condensation plate, it condenses on the condensation cover. During the condensation process of the mixed vapor, the liquid condensate gathers in the middle of the condensation cover. When it accumulates to a certain extent, it drips into the crucible through the central through hole at the bottom of the condensation plate, and then performs an evaporation-directional condensation cycle to finally achieve the separation of indium and tin. Due to the presence of the through hole, the temperature at the center of the condensation cover is higher than the surrounding temperature, resulting in the condensation and aggregation of metal indium around the condensation cover and the condensation of metal tin at the center.

[0041] like Figure 4As shown, as an embodiment of the present invention, the condensation cover in the separation device includes a top cover and an extension portion extending downwardly arranged at the center of the top cover, the inner surface of the extension portion is an arc-shaped curved surface, and is concave upward. Specifically, the entire extension portion presents a structure that is thin in the center and thick around. In the present invention, the thickness of the top cover is preferably 15mm, the thickness of the downward extension is preferably 4.8mm, the center thickness of the condensation cover is preferably 14.8mm, and the thickness around the extension portion of the condensation cover is preferably 19.8mm. The present invention provides an extension portion to achieve an interference fit between the condensation cover and the condensation tray. Figure 5 This is a top view of the condensation cover in the condensation device used in Examples 1 to 8, showing the top cover and the extension portion from a top view.

[0042] The condensation plate and the condensation cover in the separation device provided by the present invention are sealed. The sealing makes the condensation cover and the condensation plate have no gap after being combined, and then the condenser is combined with the crucible, so that the entire vacuum distillation-directional condensation process is in a closed state, achieving no metal loss and improving the direct recovery rate of indium.

[0043] The present invention also provides a method for vacuum separation and purification of indium tin lead-free solder, using the separation equipment described in the above technical solution, comprising the following steps:

[0044] Placing the indium tin lead-free solder in the crucible of the separation device for vacuum distillation to obtain a residue and volatile vapor;

[0045] The volatile vapor passes through the through holes of the condensation tray and is condensed in the condenser, thereby obtaining a metal indium product in the condensation tray and the condensation cover, and obtaining a residual metal tin product in the crucible.

[0046] In the present invention, the mass percentage of indium in the indium tin lead-free solder is preferably 48-55%, more preferably 50-52%, and the mass percentage of tin is preferably 45-52%, more preferably 48-50%.

[0047] In the present invention, the temperature during the vacuum distillation is preferably 1100-1300°C, more preferably 1150-1250°C; the distillation time is preferably 400-480 min, more preferably 420-460 min; the vacuum pressure is preferably 0.1-1 Pa, more preferably 0.3-0.8 Pa.

[0048] The present invention utilizes the difference in saturated vapor pressures of indium and tin, and through vacuum distillation, indium is volatilized into the gas phase, while tin does not volatilize or a small amount of volatilization remains in the liquid phase, thereby achieving separation of indium and tin. The obtained residue is mainly liquid phase tin, and the volatile vapor is mainly indium vapor and contains a small amount of tin vapor.

[0049] Then the volatile vapor passes through the opening of the crucible and enters the condenser from the through hole at the bottom of the condensation plate. Tin with a higher condensation temperature condenses in the condensation plate, while indium vapor continues to rise and contacts the condensation cover with a lower temperature than the condensation plate, and condenses on the condensation cover. At the same time, due to the presence of the through hole, the temperature at the center of the condensation cover is higher than the surrounding temperature, causing metal indium to condense and gather around the condensation cover, and metal tin to condense at the center. When the tin liquid accumulates to a certain extent in the middle of the condensation cover, it will drip into the crucible through the central through hole at the bottom of the condensation plate, and then perform an evaporation-directional condensation cycle to finally achieve the separation of indium and tin.

[0050] In the present invention, the purity of the metal indium product is 93-99.8%, and the purity of the metal tin product is 84-99.99%.

[0051] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described in conjunction with specific embodiments below. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Any modification, equivalent replacement, improvement, etc. made to the implementation methods of the present invention based on the technical essence and general principles of the present invention without creative work should be within the scope of protection of the present invention.

[0052] The thickness of the condensation plate in the condenser used in Examples 1 to 5 and Comparative Examples 1 to 3 is 10 mm, the depth of the condensation plate is 50 mm, the inner diameter of the condensation plate is 180 mm, a through hole is opened at the center of the bottom of the condensation plate, and a cofferdam is arranged around the through hole. The diameter of the through hole is 44 mm, the height of the cofferdam is 10 mm, the thickness of the cofferdam is 8 mm, and the inner surface of the condensation plate is an arc-shaped surface with a radius of curvature of 30 mm.

[0053] The inner surface of the condenser cover in the condenser used includes a top cover and an extension portion extending downwardly arranged at the center of the top cover. The inner surface of the extension portion is an arc-shaped curved surface and is concave upward. Specifically, the entire extension portion presents a thin center and thick surrounding structure. The difference between the center thickness and the surrounding thickness of the condenser cover is 5mm, the thickness of the top cover is 15mm, the thickness of the downward extension is 4.8mm, the center thickness of the condenser cover is 14.8mm, the thickness of the surrounding extension of the condenser cover is preferably 19.8mm, and the maximum vertical distance between the condenser cover and the condensation tray is 55mm.

[0054] Example 1

[0055] Take 30g of 52In-48Sn alloy as raw material and put it into a graphite crucible, place the condensation device on the graphite crucible, set the pressure to 0.1Pa, the temperature to 1100℃, and keep warm for 480min. After cooling, 16.66g of residue was collected in the graphite crucible, 4.46g of volatiles were collected in the condensation plate, and 8.68g of volatiles were collected on the condensation cover. ICP-MS detection: Sn: 84.68%, In: 15.32% in the residue; In: 99.54%, Sn: 0.39% in the condensation cover; In: 99.09%, Sn: 0.72% on the condensation plate.

[0056] Example 2

[0057] Take 30g of 52In-48Sn alloy as raw material and put it into a graphite crucible. Place the condensation device on the graphite crucible, set the pressure to 0.5Pa, the temperature to 1150℃, and keep warm for 460min. After cooling, 14.26g of residue was collected in the graphite crucible, 4.44g of volatiles were collected in the condensation plate, and 11.25g of volatiles were collected on the condensation cover. ICP-MS detection: Sn: 99.61% in the residue, In: 0.39%; In: 99.09% in the condensation cover, Sn: 0.91%; In: 98.93% on the condensation plate, Sn: 1.07%.

[0058] Example 3

[0059] Take 30g of 52In-48Sn alloy as raw material and put it into a graphite crucible, place the condensation device on the graphite crucible, set the pressure to 1Pa, the temperature to 1200℃, and keep warm for 440min. After cooling, the residue collected in the graphite crucible was 13.88g, the volatiles collected in the condensation plate were 4.60g, and the volatiles collected on the condensation cover were 11.22g. ICP-MS detection: Sn: 99.984%, In: 0.016% in the residue; In: 98.45%, Sn: 1.55% in the condensation cover; In: 98.37%, Sn: 1.63% on the condensation plate.

[0060] Example 4

[0061] Take 30g of 52In-48Sn alloy as raw material and put it into a graphite crucible, place the condensation device on the graphite crucible, set the pressure to 1Pa, the temperature to 1250℃, and keep warm for 420min. After cooling, the residue collected in the graphite crucible was 13.58g, the volatiles collected in the condensation plate were 4.18g, and the volatiles collected on the condensation cover were 11.84g. ICP-MS detection: Sn: 99.9905%, In: 0.0095% in the residue; In: 97.43%, Sn: 2.57% in the condensation cover; In: 95.83%, Sn: 4.27% on the condensation plate.

[0062] Example 5

[0063] Take 30g of 52In-48Sn alloy as raw material and put it into a graphite crucible, place the condensation device on the graphite crucible, set the pressure to 1Pa, the temperature to 1300℃, and keep warm for 400min. After cooling, the residue collected in the graphite crucible was 13.18g, the volatiles collected in the condensation plate were 3.36g, and the volatiles collected on the condensation cover were 13.06. ICP-MS detection: Sn: 99.9908%, In: 0.0092% in the residue; In: 95.42%, Sn: 4.58% in the condensation cover; In: 93.34%, Sn: 6.66% on the condensation plate.

[0064] Comparative Example 1

[0065] Take 30g of 52In-48Sn alloy as raw material and put it into a graphite crucible. Place the condensation device on the graphite crucible, set the pressure to 0.1Pa, the temperature to 1050℃, and keep warm for 500min. After cooling, the residue collected in the graphite crucible was 22.67g, the volatiles collected in the condensation plate were 1.800g, and the volatiles collected on the condensation cover were 5.43g. ICP-MS detection: Sn: 63.17%, In: 36.83% in the residue; In: 99.74%, Sn: 0.26% in the condensation cover; In: 99.71%, Sn: 0.29% on the condensation plate.

[0066] Comparative Example 2

[0067] Take 30g of 52In-48Sn alloy as raw material and put it into a graphite crucible, place the condensation device on the graphite crucible, set the pressure to 1Pa, the temperature to 1350℃, and keep warm for 380min. After cooling, the residue collected in the graphite crucible was 12.60g, the volatiles collected in the condensation plate were 3.42g, and the volatiles collected on the condensation cover were 13.58. ICP-MS detection: Sn: 99.9938%, In: 0.0062% in the residue; In: 93.05%, Sn: 6.95% in the condensation cover; In: 87.88%, Sn: 12.12% on the condensation plate.

[0068] Comparative Example 3

[0069] Take 30g of 52In-48Sn alloy as raw material and put it into a graphite crucible, place the condensation device on the graphite crucible, set the pressure to 1Pa, the temperature to 1400℃, and keep warm for 360min. After cooling, the residue in the graphite crucible was 11.42g, the volatiles collected in the condensation plate were 4.97g, and the volatiles collected on the condensation cover were 13.31. ICP-MS detection: Sn: 99.9954%, In: 0.0046% in the residue; In: 88.67%, Sn: 11.33% in the condensation cover; In: 76.55%, Sn: 23.45% on the condensation plate.

[0070] Comparative Example 4

[0071] Take 30g of 52In-48Sn alloy as raw material and put it into a graphite crucible without condensation device, set the pressure to 1Pa, the temperature to 1300℃, and keep warm for 400min. After cooling, the residue in the graphite crucible was 12.42g, the volatile matter was 15.23g, and the loss was 2.35g. ICP-MS detection: Sn: 99.9915%, In: 0.0085% in the residue; In: 86.03%, Sn: 13.97% in the volatile matter.

[0072] By comparing the indium and tin content in the crucible, condensation tray and condensation cover measured by Examples 1 to 5 and Comparative Examples 1 to 3, it can be seen that when the temperature is 1050°C, a small amount of vapor is volatilized, and most of the alloy remains in the crucible. At this time, the alloy in the crucible contains both indium and tin. Because the volatilization temperature of indium is low, the content of indium in the volatilization vapor is high, and the purity of indium condensed on the condensation tray and condensation cover is high, which can reach more than 99.5%. As the temperature increases, the content of tin in the volatilization vapor also gradually increases, resulting in an increase in the tin content in the condensate collected on the condensation tray and condensation cover. When the temperature increases to 1300°C, indium is almost completely converted into vapor and enters the condenser, which makes the tin content in the residue in the crucible as high as 99.99%. When the temperature is higher than 1350°C, the vapor contains both indium and tin, which increases the tin content in the condensation tray and condensation cover. When there is no condensation device, the direct recovery rate of indium is significantly reduced, the metal loss is large, and the indium content in the volatiles is low. By controlling the distillation temperature and time and using a condensation device, indium with a purity of ≥99.5% and tin with a purity of ≥99.99% can be obtained. Comparing Example 5 with Comparative Example 4, in the same distillation environment, the absence of a condensation device in Comparative Example 4 resulted in a 7.8% loss in the final product, and the In content in the obtained metal indium product was 86.03%, which was 7.31-9.39% less than the In content in the metal indium obtained by using a condensation device in Example 5.

[0073] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A separation device based on vacuum distillation, characterized in that: It comprises a vacuum distillation furnace, wherein the vacuum distillation furnace comprises a crucible for containing materials to be separated; the open end of the crucible is connected to a condenser, and the condenser comprises a condensation plate and a condensation cover; A through hole is provided at the center of the bottom of the condensation plate as a steam passage; and a cofferdam is provided around the through hole; The inner surface of the condensation cover is an arc-shaped curved surface, which is concave upwards; The condensation tray and the condensation cover are sealed together.

2. The separation device according to claim 1, characterized in that The diameter of the through hole is 40-50 mm.

3. The separation device according to claim 1, characterized in that The height of the cofferdam is 8-15 mm.

4. The separation device according to claim 1, characterized in that The condensation tray has a depth of 45 to 55 mm and an inner diameter of 160 to 200 mm.

5. The separation device according to claim 1, characterized in that The inner surface of the condensation plate is an arc-shaped surface with a curvature radius of 25 to 35 mm.

6. The separation device according to claim 1, characterized in that The maximum vertical distance between the condensation cover and the condensation tray is 50-60 mm.

7. The separation device according to claim 1, characterized in that The depth of the graphite crucible in the vacuum distillation furnace is 110-140 mm.

8. A method for vacuum separation and purification of indium tin lead-free solder, characterized in that: The separation device according to any one of claims 1 to 7 comprises the following steps: Placing the indium tin lead-free solder in the crucible of the separation device for vacuum distillation to obtain a residue and volatile vapor; The volatile vapor passes through the through holes of the condensation tray and is condensed in the condenser, thereby obtaining a metal indium product in the condensation tray and the condensation cover, and obtaining a residual metal tin product in the crucible.

9. The method according to claim 8, characterized in that The temperature during the vacuum distillation is 1100-1300° C.; The vacuum distillation time is 400 to 480 minutes; The pressure of the vacuum distillation is 0.1-1Pa.

10. The method according to claim 8, characterized in that The mass percentage of indium in the indium-tin lead-free solder is 48-55%, and the mass percentage of tin is 45-52%.

Citation Information

Cited By

  • ITO waste target recovery method

    CN120757140A