Molecular catalyst / activated carbon composite material as well as preparation method and application thereof
By using molecular catalyst/activated carbon composite materials as the positive electrode material in zinc-iodine batteries, the problems of positive electrode material dissolution and zinc negative electrode corrosion in aqueous zinc-iodine batteries are solved, the electrochemical performance and cycle life are improved, and rapid conversion of iodine active substances is achieved. and efficient use.
Patent Information
- Application Number
- CN202410978665.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The shuttle side reaction of water-based zinc-iodine batteries has the problem of dissolution of the positive electrode material and corrosion of the zinc negative electrode, low utilization rate of active iodine and slow reaction kinetics.
Molecular catalyst/activated carbon composite material is used as the positive electrode material of zinc-iodine batteries. By combining molecular catalysts such as iron phthalocyanine, nickel phthalocyanine, cobalt phthalocyanine, manganese phthalocyanine, manganese phthalocyanine, to form a sheet-like stacking structure to improve the iodine active substances. Conversion speed and utilization rate inhibit the shuttle phenomenon of polyiodine compounds.
It significantly improves the electrochemical performance of zinc-iodine batteries, improves the capacity of iodine storage and zinc storage, and prolongs the cycle life. The porous structure and high specific surface area of the material promote the adsorption and desorption kinetics of iodine ions, achieving rapid and reversible iodine activity. Material conversion.
Smart Images

Figure CN118919724A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemical energy storage, and in particular relates to a molecular catalyst / activated carbon composite material and a preparation method and application thereof. Background Art
[0002] With the substantial development of human industry, the consumption of fossil energy has increased dramatically, and the ecology of the entire earth has been greatly affected. In recent years, the intensification of the greenhouse effect has made "carbon reduction" and "carbon neutrality" the common goal of countries around the world. The application of electrochemical energy storage systems that are directly converted into electrical energy through chemical reactions runs through the entire power system of smart grids and energy Internet, and is widely used in power generation, transmission, electricity consumption and other aspects. Because zinc metal has the advantages of abundant and cheap raw materials, safe environment, and high theoretical specific capacity, aqueous zinc batteries have important application prospects in the field of large-scale energy storage (such as smart grids).
[0003] Rechargeable aqueous zinc-iodine batteries are considered to be potential energy storage systems due to their excellent energy density, low cost, and environmental friendliness. Iodine, as a reactive substance, is abundant in nature, and the conversion-type energy storage mechanism avoids lattice distortion and conversion, so it has good structural stability and cycle life. However, there are still some problems that need to be solved in aqueous zinc-iodine batteries. The shuttling side reaction of polyiodide ions will cause the dissolution of the positive electrode active material and corrosion of the zinc negative electrode. In addition, there are also problems such as low utilization of active iodine and slow reaction kinetics in the reaction process. The introduction of molecular catalysts with electrocatalytic activity, through the adsorption of polyiodide, achieves high-speed kinetics and efficient active iodine conversion, effectively improving the reversibility, utilization and kinetics of iodine / polyiodide.
[0004] In order to solve the above problems, the present invention is proposed. Summary of the invention
[0005] The present application provides an efficient aqueous zinc-iodine battery catalytic positive electrode material, thereby achieving rapid and reversible conversion of iodine active substances, improving the reaction kinetics of the system, and inhibiting problems such as dissolution of the positive electrode material and corrosion of the zinc negative electrode caused by the shuttling phenomenon of poly-iodine compounds, thereby improving the electrochemical performance of the zinc-iodine battery.
[0006] In a first aspect, the present application provides a molecular catalyst / activated carbon composite material, the composite material comprising: activated carbon and a molecular catalyst supported on the activated carbon, the molecular catalyst being selected from one or more of iron phthalocyanine, nickel phthalocyanine, cobalt phthalocyanine, and manganese phthalocyanine;
[0007] The composite material body is in a sheet-like stacking structure.
[0008] Preferably, the activated carbon surface of the composite material has molecular catalyst particles in a uniformly distributed state.
[0009] In the molecular catalyst / activated carbon composite material, the doping amount of the molecular catalyst is 1 / 7 to 1 / 2.
[0010] Doping amount: refers to the mass proportion of molecular catalyst in the composite material.
[0011] The second aspect of the present application provides a method for preparing the molecular catalyst / activated carbon composite material according to the first aspect, the preparation method comprising the following steps:
[0012] Step (1), mixing a molecular catalyst, activated carbon and a solvent to obtain a mixture;
[0013] The mixing temperature is 5 to 45°C; the molecular catalyst is selected from one or more of iron phthalocyanine, nickel phthalocyanine, cobalt phthalocyanine, manganese phthalocyanine, and zinc phthalocyanine;
[0014] In the mixture, the concentration of the molecular catalyst is 1 to 5 g / L, and the mass ratio of the molecular catalyst to the activated carbon is 1 / 6 to 1;
[0015] Step (2), stirring the mixture for 15 to 35 hours, and then separating the solid from the liquid, and the obtained solid is the composite material;
[0016] Alternatively, the mixture is stirred for 0.5 to 2 hours, and then heated in a microwave at a power of 500 to 700 W for 0.5 to 10 minutes, and the solid-liquid separation is performed, and the obtained solid is the composite material.
[0017] Preferably, the molecular catalyst and activated carbon can be mixed first and then mixed with the solvent, so that the molecular catalyst and activated carbon can be mixed more evenly, which is more conducive to the reaction.
[0018] Preferably, the solvent is selected from: water, formamide, N-methylpyrrolidone, ethanol or N,N-dimethylformamide.
[0019] Preferably, the solid-liquid separation is followed by washing and drying steps.
[0020] Preferably, the molecular catalyst is selected from one, two, three, four or five of iron phthalocyanine, nickel phthalocyanine, cobalt phthalocyanine, manganese phthalocyanine and zinc phthalocyanine.
[0021] The third aspect of the present application provides the use of the molecular catalyst / activated carbon composite material described in the first aspect as a positive electrode material for a zinc-iodine battery.
[0022] A fourth aspect of the present application provides a zinc-iodine battery, wherein the positive electrode of the zinc-iodine battery comprises the molecular catalyst / activated carbon composite material described in any one of the first aspects.
[0023] Activated carbon materials can be prepared using commercially available methods.
[0024] Preferably, the zinc-iodine battery is an aqueous zinc-iodine battery.
[0025] The fifth aspect of the present invention provides a method for preparing a zinc-iodine battery, wherein the positive electrode sheet of the zinc-ion battery is prepared by the following method: the molecular catalyst / activated carbon composite material described in any one of the first aspects is made into a slurry and coated on a current collector, and then dried in a vacuum drying oven to prepare the positive electrode sheet of the zinc-ion battery.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The molecular catalyst / activated carbon composite material prepared by the present invention has excellent electrochemical properties as a positive electrode material for zinc-iodine batteries. In the prepared zinc-iodine batteries, the iodine and zinc storage capacity reaches a specific capacity of 510 mAh / g at a low current density of 0.5 A / g, and when the current density is 20 A / g, there is still a specific capacity of 313 mAh / g (Example 14). At a current density of 2 A / g, it reaches 400 mAh / g during the first discharge process, and the capacity retention rate after 2000 reversible cycles is 90% (Example 2). This shows that the prepared assembled zinc battery has a higher specific capacity and a good cycle life.
[0028] 2. The reasons why the material of the present invention has unexpected technical effects are as follows:
[0029] 1) The use of molecular catalyst / activated carbon composite materials further improves its conductivity. The iron single atom in the iron phthalocyanine material provides a large number of energy storage active sites by adsorbing iodine ions / polyiodine compounds, thereby improving the capacity of the material. This is because the iron in the iron single atom structure exists in the valence state of divalent iron ions. Iodine ions / polyiodine compounds have strong electronegativity and will have a strong interaction with iron single atoms, thereby producing an adsorption catalytic effect;
[0030] 2) The material has a high specific surface area, and the porous structure not only provides more storage sites, which is beneficial to the improvement of material capacity, but also is beneficial to the adsorption and desorption kinetics of iodide ions on the electrode surface.
[0031] 3) In the preferred technical solution, the molecular catalyst / activated carbon composite material is prepared by microwave method. The short-time heating characteristics of microwave method are used to adjust the arrangement and stacking mode of iron phthalocyanine on the surface of activated carbon, thereby improving the catalytic activity of the composite material to iodine. The microwave method can shorten the stirring time from 15 to 35 hours to 0.5 to 2 hours.
[0032] 3. The characteristics of the preparation process of the present invention are as follows: the material is prepared by a solvent mixing method, with commercially purchased porous high specific surface area activated carbon (AC) as a carrier, and commercial iron phthalocyanine (FePC) is fully mixed in N, N-dimethylformamide solvent. During the microwave reaction, the porous activated carbon provides more sites for the doping of iron phthalocyanine, well disperses the active catalytic sites of iron single atoms, thereby avoiding the aggregation of molecular catalysts. The material preparation process is simple and has low energy consumption.
[0033] 4. The characteristics of the aqueous zinc-iodine battery assembled with the molecular catalyst / activated carbon composite material prepared by the present invention are as follows: the molecular catalyst / activated carbon composite material is made into a positive electrode sheet, and the composite material loading is 2-3 mg / cm 2 Zinc metal is used as the negative electrode, and the electrolyte is a mixed solution of 3 mol / L zinc sulfate and 0.5 mol / L potassium iodide. The KI solution in the electrolyte serves as an electrochemically active iodine source. The iron ions in the composite material doped with iron phthalocyanine, a molecular catalyst of the positive electrode, have a strong adsorption effect on iodine ions / polyiodine compounds, thereby improving the utilization rate of active iodine, promoting the conversion reversibility of iodine ions / polyiodine compounds, and improving the kinetic performance.
[0034] The porous structure and high specific surface area of the material are also conducive to the storage of iodine ions / polyiodine compounds. Through the physical confinement of the micropores, the shuttling phenomenon of polyiodine compounds is inhibited, so that the system obtains excellent and stable electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 These are scanning electron microscope images (SEM) of different metal phthalocyanine molecular catalysts / activated carbon composite materials and activated carbon obtained in Examples 3-7.
[0036] Figure 2 This is the mapping image of the molecular catalyst / activated carbon composite material obtained in Example 3.
[0037] Figure 3 This is the mapping image of the molecular catalyst / activated carbon composite material obtained in Example 4.
[0038] Figure 4 This is the mapping image of the molecular catalyst / activated carbon composite material obtained in Example 5.
[0039] Figure 5 This is the mapping image of the molecular catalyst / activated carbon composite material obtained in Example 6.
[0040] Figure 6 This is the mapping image of the molecular catalyst / activated carbon composite material obtained in Example 7.
[0041] Figure 7 This is a long cycle diagram of the molecular catalyst / activated carbon composite material obtained in Example 3-7 as the positive electrode of a zinc battery.
[0042] Figure 8 This is a long cycle diagram of the molecular catalyst / activated carbon composite material obtained in Examples 3, 8-11 as the positive electrode of a zinc battery.
[0043] Fig. 9 This is a long cycle diagram of the molecular catalyst / activated carbon composite material of Examples 1-3 as the positive electrode of a zinc battery.
[0044] Fig.10 The graphs are differential capacitance curves of the molecular catalyst / activated carbon composite materials and activated carbon of Examples 1-3 as the positive electrode of zinc batteries, respectively.
[0045] Fig.11 The XRD patterns of the molecular catalyst / activated carbon composite material, iron phthalocyanine and activated carbon obtained in Examples 1-3 are shown.
[0046] Fig.12 Scanning electron microscope (SEM) images of the molecular catalyst / activated carbon composite material and activated carbon obtained in Examples 12-17.
[0047] Fig.13 This is a long cycle diagram of the molecular catalyst / activated carbon composite material obtained in Examples 12-17 as the positive electrode of a zinc battery.
[0048] Fig.14 The differential capacitance curves of the molecular catalyst / activated carbon composite materials obtained in Examples 12-17 as the positive electrode of the zinc battery are shown.
[0049] Fig.15 This is a rate performance diagram of the molecular catalyst / activated carbon composite material obtained in Example 14 as a positive electrode of a zinc battery. DETAILED DESCRIPTION
[0050] The present invention is described below in conjunction with specific examples, but the embodiments of the present invention are not limited thereto. Experimental methods without specific conditions in the examples are usually carried out according to conventional conditions and conditions described in the manual, or according to the conditions recommended by the manufacturer. The general equipment, materials, reagents, etc. used can be obtained from commercial channels unless otherwise specified. The raw materials required in the following examples and comparative examples are all commercially available.
[0051] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0052] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution. If not otherwise specified, all technical features and optional technical features of the present application can be combined with each other to form a new technical solution. If not otherwise specified, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0053] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0054] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B".
[0055] The molecular catalysts (ferron phthalocyanine, nickel phthalocyanine, cobalt phthalocyanine, manganese phthalocyanine, zinc phthalocyanine) and activated carbon (AC) materials in the embodiments can be purchased commercially.
[0056] The aqueous zinc-iodine battery assembled with the molecular catalyst / activated carbon composite material prepared in the embodiment of the present invention is assembled as follows: the prepared molecular catalyst / activated carbon composite material is made into a positive electrode sheet, and the active composite material loading is 2-3 mg / cm 2 , zinc metal is the negative electrode, and the electrolyte is a mixed solution of 3 mol / L zinc sulfate and 0.5 mol / L potassium iodide.
[0057] Example 1
[0058] The molecular catalyst / activated carbon composite cathode material prepared by non-microwave method is prepared by the following method:
[0059] 10 mg of iron phthalocyanine (FePC) and 60 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was room temperature 20°C, and the stirring time was 20 hours. After stirring, the mixture was taken out, centrifuged, washed, and dried to obtain a composite material. In the molecular catalyst / activated carbon composite material, the molecular catalyst doping amount was 1 / 7.
[0060] Example 2
[0061] The molecular catalyst / activated carbon composite cathode material prepared by non-microwave method is prepared by the following method:
[0062] 10 mg of iron phthalocyanine (FePC) and 20 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was room temperature 20°C, and the stirring time was 20 h. After stirring, the mixture was taken out, centrifuged, washed, and dried to obtain a composite material.
[0063] Example 3
[0064] The molecular catalyst / activated carbon composite cathode material prepared by non-microwave method is prepared by the following method:
[0065] 10 mg of iron phthalocyanine (FePC) and 10 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was room temperature 20°C, and the stirring time was 20 hours. After stirring, the mixture was taken out, centrifuged, washed, and dried to obtain a composite material. In the molecular catalyst / activated carbon composite material, the molecular catalyst doping amount was 1 / 2.
[0066] Example 4
[0067] The molecular catalyst / activated carbon composite cathode material prepared by non-microwave method is prepared by the following method:
[0068] 10 mg of nickel phthalocyanine (NiPC) and 10 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was room temperature 20°C, and the stirring time was 20 h. After stirring, the mixture was taken out, centrifuged, washed, and dried to obtain a composite material.
[0069] Example 5
[0070] The molecular catalyst / activated carbon composite cathode material prepared by non-microwave method is prepared by the following method:
[0071] 10 mg of cobalt phthalocyanine (CoPC) and 10 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was room temperature 20°C, and the stirring time was 20 h. After stirring, the mixture was taken out, centrifuged, washed, and dried to obtain a composite material.
[0072] Example 6
[0073] The molecular catalyst / activated carbon composite cathode material prepared by non-microwave method is prepared by the following method:
[0074] 10 mg of zinc phthalocyanine (ZnPC) and 10 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was room temperature 20°C, and the stirring time was 20 h. After stirring, the mixture was taken out, centrifuged, washed, and dried to obtain a composite material.
[0075] Example 7
[0076] The molecular catalyst / activated carbon composite cathode material prepared by non-microwave method is prepared by the following method:
[0077] 10 mg of manganese phthalocyanine (MnPC) and 10 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was room temperature 20°C, and the stirring time was 20 h. After stirring, the mixture was taken out, centrifuged, washed, and dried to obtain a composite material.
[0078] Example 8
[0079] The molecular catalyst / activated carbon composite cathode material prepared by non-microwave method is prepared by the following method:
[0080] 10 mg of iron phthalocyanine (FePC) and 10 mg of activated carbon were mixed evenly, and further mixed in 10 mL of deionized water, wherein the mixing temperature was 45° C. and the stirring time was 15 h. After stirring, the mixture was taken out, centrifuged, washed, and dried to obtain a composite material.
[0081] Example 9
[0082] The molecular catalyst / activated carbon composite cathode material prepared by non-microwave method is prepared by the following method:
[0083] 10 mg of iron phthalocyanine (FePC) and 10 mg of activated carbon were mixed evenly, and further mixed in 10 mL of formamide solvent, wherein the mixing temperature was 5° C. and the stirring time was 35 h. After stirring, the mixture was taken out, centrifuged, washed, and dried to obtain a composite material.
[0084] Example 10
[0085] The molecular catalyst / activated carbon composite cathode material prepared by non-microwave method is prepared by the following method:
[0086] 10 mg of iron phthalocyanine (FePC) and 10 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N-methylpyrrolidone solvent, wherein the mixing temperature was room temperature 20° C., and the stirring time was 20 h. After stirring, the mixture was taken out, centrifuged, washed, and dried to obtain a composite material.
[0087] Embodiment 11
[0088] The molecular catalyst / activated carbon composite cathode material prepared by non-microwave method is prepared by the following method:
[0089] 10 mg of iron phthalocyanine (FePC) and 10 mg of activated carbon were mixed evenly, and further mixed in 10 mL of ethanol, wherein the mixing temperature was room temperature 20° C., and the stirring time was 20 h. After stirring, the mixture was taken out, centrifuged, washed, and dried to obtain a composite material.
[0090] Example 12
[0091] The preparation method of the molecular catalyst / activated carbon composite positive electrode material prepared by microwave method is as follows:
[0092] 10 mg of iron phthalocyanine and 20 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was room temperature 20°C, and the stirring time was 0.5 h. After stirring, the mixture was heated in a microwave at a power of 500 W for 20 min, taken out, centrifuged, washed, and dried to obtain a composite material.
[0093] Embodiment 13
[0094] The preparation method of the molecular catalyst / activated carbon composite positive electrode material prepared by microwave method is as follows:
[0095] 10 mg of iron phthalocyanine, 10 mg of manganese phthalocyanine and 40 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was room temperature 20°C, and the stirring time was 1 hour. After stirring, the mixture was heated in a microwave at a power of 600 W for 3 minutes, taken out, centrifuged, washed and dried to obtain a composite material.
[0096] Embodiment 14
[0097] The preparation method of the molecular catalyst / activated carbon composite positive electrode material prepared by microwave method is as follows:
[0098] 10 mg of iron phthalocyanine, 10 mg of cobalt phthalocyanine and 40 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was 28°C and the stirring time was 2 h. After stirring, the mixture was heated in a microwave at a power of 700 W for 0.5 min, taken out, centrifuged, washed and dried to obtain a composite material.
[0099] Embodiment 15
[0100] The preparation method of the molecular catalyst / activated carbon composite positive electrode material prepared by microwave method is as follows:
[0101] 10 mg of iron phthalocyanine, 5 mg of nickel phthalocyanine, 5 mg of zinc phthalocyanine and 40 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was 28°C and the stirring time was 2 h. After stirring, the mixture was heated in a microwave at a power of 700 W for 3 min, taken out, centrifuged, washed and dried to obtain a composite material.
[0102] Example 16
[0103] The preparation method of the molecular catalyst / activated carbon composite positive electrode material prepared by microwave method is as follows:
[0104] 8 mg of iron phthalocyanine, 4 mg of nickel phthalocyanine, 4 mg of manganese phthalocyanine, 4 mg of zinc phthalocyanine and 40 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was 28°C, and the stirring time was 2 h. After stirring, the mixture was heated in a microwave at a power of 700 W for 3 min, taken out, and centrifuged, washed and dried to obtain a composite material.
[0105] Embodiment 17
[0106] The preparation method of the molecular catalyst / activated carbon composite positive electrode material prepared by microwave method is as follows:
[0107] 20 mg of iron phthalocyanine, 5 mg of nickel phthalocyanine, 5 mg of manganese phthalocyanine, 5 mg of zinc phthalocyanine, 5 mg of cobalt phthalocyanine and 40 mg of activated carbon were mixed evenly, and further mixed in 10 mL of N,N-dimethylformamide solvent, wherein the mixing temperature was 28°C, and the stirring time was 2 h. After stirring, the mixture was heated in a microwave at a power of 700 W for 3 min, taken out, and centrifuged, washed and dried to obtain a composite material.
[0108] Figure 1 The scanning electron microscope (SEM) images of different metal phthalocyanine molecular catalysts / activated carbon composite materials and activated carbon obtained in Examples 3 to 7. By comparing the SEM images of activated carbon (AC) and the composite materials, it can be seen that different metal phthalocyanine molecular catalysts are successfully loaded on AC, and different metal phthalocyanine molecular catalysts present nanoparticle morphology and are evenly distributed on the surface of AC.
[0109] Figure 2-6 The mapping images of the molecular catalyst / activated carbon composite materials obtained in Examples 3 to 7 are shown in turn. It can be seen from the images that FePc, NiPc, CoPc, ZnPc, and MnPc molecular catalysts are successfully loaded on AC, and the doping is relatively uniform, which provides good catalytic sites for the catalytic conversion of iodine ions / polyiodine compounds.
[0110] Figure 7 The long cycle diagram of different metal phthalocyanine molecular catalysts / activated carbon composite materials used as zinc battery positive electrodes in Examples 3-7, the minimum current density used for constant current charge and discharge is 2A / g, where the horizontal axis is the number of cycles; the vertical axis is the specific capacity, unit: milliampere-hour / gram. By comparison, the molecular catalyst / activated carbon composite materials obtained when FePC, NiPC, CoPC, ZnPC, and MnPC are used as raw materials are used as positive electrodes, and the initial specific capacities are 400, 370, 260, 180, and 370 mAh / g, respectively, and the capacity retention rates are 90% (2000 cycles), 86% (short circuit after 300 cycles), 77% (short circuit after 800 cycles), 55.5% (short circuit after 710 cycles), and 27% (700 cycles). Among them, the molecular catalyst / activated carbon composite material corresponding to FePC has the best specific capacity and cycle performance.
[0111] Figure 8The long cycle diagram of the iron phthalocyanine molecular catalyst / activated carbon composite material prepared in different solvents in Examples 3, 8-11 as the positive electrode of the zinc battery, the current density used for constant current charge and discharge is 2A / g, where the horizontal axis is the number of cycles; the vertical axis is the specific capacity, unit: milliampere-hour / gram. By comparison, the molecular catalyst / activated carbon composite material obtained when water, formamide, N-methylpyrrolidone, ethanol, and N,N-dimethylformamide are used as solvents as the positive electrode has an initial specific capacity of 280, 305, 330, 270, and 400 mAh / g, respectively, and the capacity retention rate is 44.4% (710 cycles), 65% (short circuit after 1350 cycles), 78.79% (short circuit after 910 cycles), 40% (short circuit after 800 cycles), and 90% (2000 cycles). Among them, the molecular catalyst / activated carbon composite material corresponding to N,N-dimethylformamide has the best specific capacity and cycle performance.
[0112] Fig. 9 The figure is a long cycle diagram of the molecular catalyst / activated carbon composite material of Examples 1-3 as the positive electrode of the zinc battery. The small current density used for constant current charge and discharge is 2A / g, wherein the horizontal axis is the number of cycles; the vertical axis is the specific capacity, unit: mAh / g. By comparison, the molecular catalyst / activated carbon composite material obtained in Examples 1-3 is used as the positive electrode, and the initial specific capacities of Examples 2, 1, and 3 are 400, 310, and 260 mAh / g, respectively, and the capacity retention rates are 90% (2000 cycles), 80% (2000 cycles), and 77% (short circuit after 520 cycles), respectively, which are all higher than the activated carbon positive electrode. The zinc battery assembled therefrom has a higher specific capacity and a good cycle life.
[0113] Fig.10 The differential capacitance curves of the molecular catalyst / activated carbon composite material and activated carbon of Examples 1-3 as the positive electrode of the zinc battery, respectively, are shown in Figure 1-3. The current density used for constant current charging and discharging is 2A / g, respectively. The horizontal axis is voltage, unit: volt; the vertical axis is differential capacitance, unit: milliampere-hour / volt. It can be seen from the differential capacitance curve that the reactive substance in the battery is iodine, and as the FePC doping ratio increases, a reduction peak with a discharge voltage of 1.3V appears, indicating that during the reaction, compared with the activated carbon positive electrode, each I ion at 1.15V transfers 2 / 3 of the electrons of I - / I3 - In terms of the reaction, there is also I in the composite material with single electron transfer - / I2 reaction is the main one, which proves the catalytic conversion of I by the composite catalytic material.
[0114] Fig.11The XRD diagrams of the molecular catalyst / activated carbon composite material, iron phthalocyanine and activated carbon obtained in Examples 1-3. Through XRD characterization analysis, it was found that when the FePc doping amount was small, that is, FePc:AC=1:6 and 1:2, the material had no fixed crystal form. When FePc:AC=1:1, a trace amount of FePc signal appeared in XRD characterization. It proves that as the FePc doping amount increases, the FePc crystal phase appears on the AC surface, which also proves the successful doping of FePc.
[0115] Fig.12 The SEM images of the molecular catalyst / activated carbon composite material and activated carbon obtained in Examples 12 to 17 are shown in Figure 1. By comparing the SEM images of activated carbon (AC) and the composite material, it can be seen that the molecular catalyst is successfully loaded on AC, and as the mixed species of the molecular catalyst are adjusted, the molecular catalyst presents a nanoparticle accumulation morphology on the AC surface.
[0116] Fig.13 The long cycle diagram of the molecular catalyst / activated carbon composite material obtained in Examples 12-17 as the positive electrode of the zinc battery, the small current density used for constant current charge and discharge is 2A / g, wherein the horizontal axis is the number of cycles; the vertical axis is the specific capacity, unit: milliampere hour / gram. By comparison, the molecular catalyst / activated carbon composite material obtained in Examples 12-14 is used as the positive electrode, the initial specific capacity is 300, 500, 390mAh / g, respectively, and the capacity retention rate after 2000 reversible cycles is 67%, 40%, 85%, respectively. The molecular catalyst / activated carbon composite material obtained in Example 15 is used as the positive electrode, the initial specific capacity is 500mAh / g, respectively, and the capacity retention rate after 600 reversible cycles is 45%, respectively. The molecular catalyst / activated carbon composite material obtained in Examples 16-17 is used as the positive electrode, the initial specific capacity is 500, 510mAh / g, respectively, and the capacity retention rate after 1100 reversible cycles is 45%, 35%, respectively. The assembled zinc battery has a high specific capacity and a good cycle life.
[0117] Fig.14 The differential capacitance curves of the molecular catalyst / activated carbon composite materials obtained in Examples 12-17 as the positive electrode of the zinc battery are shown in Figure 12-17. The current density used for constant current charging and discharging is 2A / g, respectively. The horizontal axis is voltage, unit: volt; the vertical axis is differential capacitance, unit: milliampere-hour / volt. It can be seen from the differential capacitance curve that the reactive substance in the battery is iodine. Compared with only FePC molecular catalyst, as FePC is doped with NiPc, CoPc, ZnPc, MnPc, etc., the reduction peak with a discharge voltage of 1.3V is more obvious, indicating that the I ion transfers 2 / 3 electrons compared to the I ion transfer at 1.15V during the reaction. - / I3 - In terms of the reaction, this system mainly uses single electron transfer I- / I2 reaction is the main reaction, which proves the high efficiency of the composite catalytic material in catalytic conversion of I. And the redox peak voltage difference is small, only 30mv, indicating that the battery has high reversibility and high reversibility of I conversion.
[0118] Fig.10 and Fig.14 The comparison shows that the proportion of single electron transfer reaction of the composite material designed by microwave method is significantly higher than that of the composite material stirred at room temperature and that of the composite material without microwave method, which proves that microwave method has a significant improvement on the catalytic performance of the composite material. That is, the microwave process has further improved the catalytic performance of the composite material during the reaction. - Due to the catalytic effect of / I2 reaction, the proportion of single electron transfer reaction is significantly increased, thereby improving the capacity, and the good rate performance also proves the improvement of reaction kinetics.
[0119] Fig.15 This is a rate performance diagram of the molecular catalyst / activated carbon composite material obtained in Example 14 as the positive electrode of a zinc battery. The current density used for constant current charge and discharge is 0.3, 0.5, 1, 2, 3, 4, 5, 7, 10, and 20 A / g, where the horizontal axis is the number of cycles; the vertical axis is the specific capacity, unit: mAh / g. Fig.15 This shows that the composite material of Example 14 has good rate performance as the positive electrode of the zinc battery, with a specific capacity of 510 mAh / g at a low current density of 0.5 A / g, and a specific capacity of 313 mAh / g at a current density of 20 A / g. The capacity retention rate is 61.4%.
Claims
1. A molecular catalyst / activated carbon composite material, It is characterized in that The composite material comprises: activated carbon and a molecular catalyst supported on the activated carbon, wherein the molecular catalyst is stacked on the activated carbon in the form of nanoparticles; The molecular catalyst is selected from one or more of iron phthalocyanine, nickel phthalocyanine, cobalt phthalocyanine, manganese phthalocyanine and zinc phthalocyanine.
2. The composite material according to claim 1, It is characterized in that In the composite material, the doping amount of the molecular catalyst is 1 / 7 to 1 / 2, and the doping amount refers to the mass proportion of the molecular catalyst in the composite material.
3. The composite material according to claim 1, It is characterized in that The molecular catalyst is uniformly distributed on the activated carbon.
4. A method for preparing the molecular catalyst / activated carbon composite material according to claim 1, It is characterized in that The preparation method comprises the following steps: Step (1), mixing a molecular catalyst, activated carbon and a solvent to obtain a mixture; The mixing temperature is 5 to 45°C; the molecular catalyst is selected from one or more of iron phthalocyanine, nickel phthalocyanine, cobalt phthalocyanine, manganese phthalocyanine, and zinc phthalocyanine; In the mixture, the total concentration of the molecular catalyst and the activated carbon is 2 to 7 g / L, and the mass ratio of the molecular catalyst to the activated carbon is 1 / 6 to 1; Step (2), stirring the mixture for 15 to 35 hours, and then separating the solid from the liquid, and the obtained solid is the composite material; Alternatively, the mixture is stirred for 0.5 to 2 hours, and then heated by microwave at a power of 500 to 700 W for 0.5 to 20 minutes, and the solid and liquid are separated, and the obtained solid is the composite material.
5. The preparation method according to claim 4, It is characterized in that The solvent is selected from: water, formamide, N-methylpyrrolidone, ethanol or N,N-dimethylformamide.
6. A zinc-iodine battery, It is characterized in that The positive electrode of the zinc-iodine battery comprises the molecular catalyst / activated carbon composite material according to any one of claims 1 to 3.
7. Use of the molecular catalyst / activated carbon composite material according to any one of claims 1 to 3 as a positive electrode material for zinc-iodine batteries.
Citation Information
Patent Citations
Composite material based on metal phthalocyanine compound and carbon and application of composite material in lithium-sulfur battery
CN110010857A
Method for preparing heterogeneous monomolecular electrocatalyst from metal phthalocyanine molecule-nanocarbon and application of heterogeneous monomolecular electrocatalyst
CN110911694A
Carbon composite material chemically modified by metal phthalocyanine complex, battery cathode material and preparation method and application thereof
CN111450888A
Solid electrolyte cell and iodine-doped metal complexes as the cathode material
US4584251A
Composite catalyst for removing mercaptans from liquids and gasses
WO1995015215A1
Cited By
Inorganic / organic hybrid material synergistically stable zinc-iodine battery and application thereof
CN119481360A
A zinc-iodine battery synergistically stabilized by an inorganic / organic hybrid material and its application
CN119481360B
Composite positive electrode based on synergistic oxidation reduction of metal phthalocyanine and iodine, preparation method and battery
CN122455636A
A composite positive electrode based on metal phthalocyanine and iodine synergistic oxidation-reduction, a preparation method and a battery
CN122455636B