Anti-ferroelectric artificial nerve device and preparation method thereof

By forming a hafnium zirconium oxide film on the substrate and performing rapid heat treatment, high-performance antiferroelectric artificial neuron devices were prepared, which solved the problem that existing ferroelectric devices were difficult to simulate the potential changes of biological neurons, and achieved spontaneous extremes The functions of state switching and neuron accumulation, excitation, and self-recovery simplify the process and reduce costs.

CN118922057APending Publication Date: 2024-11-08FUDAN UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410974686.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Due to its inherent nonvolatile characteristics, existing ferroelectric artificial neuron devices are difficult to simulate the transient potential changes of biological neurons, and additional feedback paths are required to achieve spontaneous reset after excitation, and the complex process increases hardware cost and work. Consumption.

Method used

By forming a thin film of hafnium zirconium oxide on the substrate and crystallizing it through rapid heat treatment to produce antiferroelectricity, combined with physical meteorological deposition and wet etching technology, high-performance antiferroelectric artificial neuron devices are prepared. Implement spontaneous polarization state switching and neuronal accumulation, excitation and self-recovery functions.

Benefits of technology

The process is simplified, production costs are reduced, and the preparation of high-performance antiferroelectric artificial neuron devices is realized, which supports dynamic learning and memory functions, reduces the cost and energy consumption of neuron reset, and simulates the characteristics of biological neurons.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922057A_ABST
    Figure CN118922057A_ABST
Patent Text Reader

Abstract

The invention provides an anti-ferroelectric artificial nerve component and a preparation method thereof. The preparation method comprises the following steps: providing a substrate; forming a first metal layer on the substrate as a first electrode; forming a hafnium zirconium oxide thin film on the first metal layer; forming a second metal layer on the hafnium zirconium oxide thin film; the hafnium zirconium oxide thin film is crystallized and antiferroelectricity is generated through rapid heat treatment; removing the second metal layer; and forming a third metal layer on the hafnium zirconium oxide film as a second electrode. The method has the beneficial effects that a neuron accumulation / leakage function can be realized, extra hardware and operation cost is avoided, basic neuron characteristics including accumulation, excitation and self-recovery are further realized, and biological neuron characteristics can be simulated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of artificial neuron devices, and in particular to an antiferroelectric artificial neuron device and a preparation method thereof. Background Art

[0002] When building artificial neural network hardware systems, choosing the right materials is crucial because it directly affects the performance, energy consumption, and feasibility of the system. HfO2 (hafnium oxide)-based ferroelectric materials have been widely studied for their compatibility in complementary metal oxide semiconductor (CMOS) processes and superior electrical properties for the manufacture of non-volatile memory elements, such as FeFETs (ferroelectric field effect transistors), which can mimic the threshold firing behavior of neurons.

[0003] However, the inherent non-volatility of ferroelectric materials means that once polarized, their state remains unchanged unless a reverse voltage is applied, which does not fully match the transient potential changes of biological neurons. An additional feedback path is required to achieve spontaneous reset after excitation, and the process is complex, which increases hardware costs, power consumption and operational complexity. Summary of the invention

[0004] The purpose of the present invention is to propose an antiferroelectric artificial neuron device and a preparation method thereof which can realize the basic characteristics of artificial neurons, including accumulation, excitation and self-recovery.

[0005] The present invention provides a method for preparing an antiferroelectric artificial neuron device, comprising: providing a substrate; forming a first metal layer on the substrate as a first electrode; forming a hafnium zirconium oxide film on the first metal layer; forming a second metal layer on the hafnium zirconium oxide film; crystallizing the hafnium zirconium oxide film by rapid thermal treatment and generating antiferroelectricity; removing the second metal layer; A third metal layer is formed on the hafnium zirconium oxide film to serve as a second electrode.

[0006] The method of the present invention has the following beneficial effects: by providing a flexible substrate; by providing a substrate; forming a first metal layer on the substrate as a first electrode; forming a hafnium zirconium oxide film on the first metal layer; forming a second metal layer on the hafnium zirconium oxide film; and performing an etching process on the second metal layer, the production cost is reduced, the process is simplified, and the preparation of a high-performance antiferroelectric artificial neuron device is achieved, meeting the needs of artificial neuron devices.

[0007] Furthermore, providing the substrate includes: cleaning the substrate by an RCA cleaning process, and then drying the substrate with nitrogen.

[0008] Further, a first metal layer is formed on the substrate as a first electrode, including: depositing the first metal layer using a physical vapor deposition method, wherein the first metal layer has a thickness of 80 nm.

[0009] Further, forming a hafnium zirconium oxide film on the first metal layer includes: using plasma atomic layer deposition to deposit the hafnium zirconium oxide film, at a reaction temperature of 250° C., and at a deposition rate of 0.1 nm per cycle.

[0010] Furthermore, plasma atomic layer deposition is used to deposit a hafnium zirconium oxide film, including: during the deposition process, each time a hafnium source gas is introduced for a deposition cycle, the zirconium source gas is introduced nine times in succession for deposition cycles, and the deposition thickness of the hafnium zirconium oxide film is 6 nm.

[0011] Further, forming a second metal layer on the hafnium zirconium oxide film includes: depositing the second metal layer using physical vapor deposition, wherein the second metal layer is deposited to a thickness of 80 nm.

[0012] Furthermore, after the second metal layer was deposited by physical vapor deposition, the antiferroelectric artificial neuron device was treated at 550° C. for 30 seconds by rapid thermal processing technology.

[0013] Further, removing the second metal layer includes: etching the second metal layer using a wet etching process, and the composition ratio of the wet etching solution is: .

[0014] Further, forming a third metal layer on the hafnium zirconium oxide film as the second electrode includes: depositing an 80 nm third metal layer on the hafnium zirconium oxide film using physical vapor deposition.

[0015] In some embodiments, an antiferroelectric artificial neuron device is also provided, which is manufactured using the method described in the above embodiment and includes a substrate, a first metal layer, a hafnium zirconium oxide film and a third metal layer arranged in sequence.

[0016] Furthermore, the thickness of the first metal layer is 80 nm, the thickness of the hafnium zirconium oxide film is 6 nm, the thickness of the second metal layer is 80 nm, and the thickness of the third metal layer is 80 nm.

[0017] The beneficial effects of the present invention are as follows: antiferroelectric materials can spontaneously switch between positive and negative polarization states under specific conditions, and this property enables them to simulate the process of accumulation and release of potential of neurons, thereby better supporting dynamic learning and memory functions; utilizing the intrinsic polarization reversal mechanism of HZO antiferroelectric materials, the hardware structure required for neuromorphic computing can be simplified, the cost and energy consumption required to achieve neuron resetting can be reduced, and it is helpful to develop more efficient and energy-saving neuromorphic computing chips. In addition, as an extension of HfO2-based ferroelectric materials, HZO antiferroelectric materials have strong durability, minimal incremental leakage current under electric field cycles and lower power consumption (due to lower Ec), and are another emerging system of HfO2-based ferroelectric materials. HZO antiferroelectric materials have intrinsic polarization / depolarization characteristics, which can realize neuron accumulation / leakage functions, avoid additional hardware and operating costs, and thus realize basic neuron characteristics including accumulation, excitation and self-recovery, and can simulate biological neuron characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic diagram of the structure of the present invention in a substrate-providing state; Figure 2 A schematic diagram of the structure in the first metal layer state is generated for the present invention; Figure 3 It is a schematic diagram of the structure of the present invention in which a hafnium zirconium oxide thin film is formed on the first metal layer; Figure 4 It is a schematic structural diagram of the present invention in a state where a second metal layer is formed on a hafnium zirconium oxide film; Figure 5 It is a schematic diagram of the structure of the present invention after the second metal layer is subjected to an etching process; Figure 6 It is a schematic structural diagram of the present invention after a third metal layer is formed on the hafnium zirconium oxide film; Figure 7 It is a schematic diagram of the preparation method of the present invention; Figure 8 It is a schematic diagram of the present invention when used. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise defined, the technical terms or scientific terms used herein should be understood by people with general skills in the field to which the present invention belongs. "Including" and similar words used in this article mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.

[0020] As attached Figure 1 and Figure 7 As shown, the invention proposes a method for preparing an antiferroelectric artificial neuron device, comprising: S101, providing a substrate; Specifically, a SiO2 / Si substrate 1 can be used. The SiO2 / Si substrate 1 is a composite substrate 1 composed of silicon dioxide (SiO2) and silicon (Si), and refers to a composite material in which a layer of silicon dioxide (SiO2) thin film is formed on the surface of a silicon (Si) wafer by chemical vapor deposition (CVD), thermal oxidation or wet oxidation as an insulating layer.

[0021] In some specific embodiments, providing the substrate 1 includes: performing an RCA cleaning process on the substrate 1, and then drying the substrate 1 with nitrogen gas.

[0022] Specifically, in the semiconductor manufacturing process, cleaning the substrate 1 (e.g., SiO2 / Si substrate 1) is a very important step to remove organic matter, particulate contaminants, and other impurities on the surface to ensure that the subsequently deposited thin film has excellent adhesion and purity; In addition, RCA cleaning is a classic semiconductor cleaning process, which mainly includes two steps: sulfuric acid-hydrofluoric acid mixed solution cleaning (SC-1) and ammonium hydroxide-hydrogen peroxide-water mixed solution cleaning (SC-2); After cleaning, in order to prevent contamination by impurities again, high-purity nitrogen is usually used to blow dry the substrate 1. As an inert gas, nitrogen is not easy to react with other substances and can effectively blow away moisture from the surface of the substrate 1 without introducing new pollution sources. Nitrogen drying is generally performed in a drying cabinet, and the nitrogen flow directed toward the surface of the substrate 1 quickly removes moisture to achieve the purpose of rapid drying while avoiding the risk of secondary contamination caused by natural drying.

[0023] S102, forming a first metal layer on the substrate as a first electrode; In some specific embodiments, forming a first metal layer 2 on a substrate 1 as a first electrode includes: depositing the first metal layer 2 using a physical vapor deposition method.

[0024] Specifically, physical vapor deposition (PVD) is a technique for depositing a thin film on a substrate 1 , which generally involves converting a material from a solid state to a gas state (evaporation or sputtering), and then condensing it on the substrate 1 to form a first metal layer 2 thin film.

[0025] In some specific embodiments, the thickness of the first metal layer 2 is 80 nm.

[0026] S103, forming a hafnium zirconium oxide thin film on the first metal layer; In some specific embodiments, forming the hafnium zirconium oxide film 3 on the first metal layer 2 includes: depositing the hafnium zirconium oxide film 3 using a plasma atomic layer deposition method.

[0027] Specifically, in the semiconductor manufacturing process, the formation of the Hafnium Zirconium Oxide (HZO) film on the first metal layer 2 can be achieved by plasma enhanced atomic layer deposition (PEALD) technology. PEALD is a very precise thin film growth technology that deposits atomic-level thin films layer by layer through a series of self-limiting chemical reaction steps to achieve extremely high-precision control of film thickness and composition. HZO antiferroelectric materials have intrinsic polarization / depolarization properties, which can realize neuron accumulation / leakage functions, avoid additional hardware and operating costs, and thus realize basic neuron properties including accumulation, excitation and self-recovery, and can simulate biological neuron properties.

[0028] In some specific embodiments, when the reaction temperature is 250° C., the deposition rate is 0.1 nm per cycle.

[0029] In some specific embodiments, plasma atomic layer deposition is used to deposit the hafnium zirconium oxide film 3, including: during the deposition process, after each hafnium source gas is introduced for a deposition cycle, the zirconium source gas is continuously introduced for nine deposition cycles, and the deposition thickness of the hafnium zirconium oxide film 3 is 6nm.

[0030] Specifically, in semiconductor device manufacturing, in order to obtain hafnium zirconium oxide (HZO) thin films with antiferroelectric properties, the plasma atomic layer deposition (PEALD) method is used to accurately control the composition and structure of the film. For the case where the film thickness is required to be 6nm and the deposition rate is 0.1nm / cycle; Since the film needs to be deposited to a thickness of 6nm, and each cycle deposits 0.1nm, the total number of cycles required in theory is 6nm divided by 0.1nm / time, that is: Total number of cycles = 6nm / 0.1nm / time = 60 times; In addition, in order to give the film antiferroelectric properties, it is necessary to precisely control the ratio of hafnium (Hf) and zirconium (Zr), which is set here to 1:9, meaning that during the deposition process, one cycle out of every 10 cycles is dedicated to depositing hafnium oxide, and the remaining 9 cycles are used to deposit zirconium oxide, ensuring that the ratio of elements in the final film meets the requirements, thereby preparing a 6nm thick HZO film with excellent antiferroelectric properties and suitable for storage applications on the first metal layer 2.

[0031] S104, forming a second metal layer on the hafnium zirconium oxide film; S105, crystallizing the hafnium zirconium oxide thin film and generating antiferroelectricity by rapid thermal treatment; In some specific embodiments, a second metal layer 4 is formed on the hafnium zirconium oxide film 3, including: depositing the second metal layer 4 using physical vapor deposition, the second metal layer 4 is deposited to a thickness of 80 nm, and after depositing the second metal layer 4 using physical vapor deposition, treating the antiferroelectric artificial neuron device at 550°C for 30 seconds using rapid thermal processing technology.

[0032] Specifically, a second metal layer 4 is deposited on the HZO film by physical vapor deposition (PVD). The thickness of the metal layer is set to 80 nm. In addition, this step requires precise control of deposition conditions, such as sputtering power, gas pressure, deposition time, etc., to ensure that the thickness of the metal layer is uniform and has good adhesion to the HZO film. In implementation, the material of the second metal layer 4 is usually selected to be a metal with good conductivity, compatible with the HZO film and capable of meeting the functional requirements of the device, such as platinum (Pt), aluminum (Al), copper (Cu), etc.

[0033] After the deposition of the second metal layer 4 is completed, the entire antiferroelectric artificial neuron device is heat treated using rapid thermal processing technology. In this case, the device will be placed in a specific high temperature environment and heat treated at 550°C for 30 seconds. The main purpose of the rapid thermal treatment is to produce a good interface reaction between the second metal layer 4 and the HZO film and improve the adhesion strength between them. It may also help to improve the antiferroelectric properties of the HZO film and activate the potential charge storage mechanism.

[0034] S106, removing the second metal layer; In some specific embodiments, removing the second metal layer includes: etching the second metal layer using a wet etching process, and the composition ratio of the wet etching solution is as follows: .

[0035] Specifically, wet etching uses chemical solutions to react with the metal layer to selectively remove unnecessary parts to form a desired pattern, and uses the principle that the thermal expansion coefficients of the second metal layer 4 and the antiferroelectric layer are different to crystallize the HZO film and generate antiferroelectricity.

[0036] S107, forming a third metal layer on the hafnium zirconium oxide film as a second electrode.

[0037] In some specific embodiments, forming a third metal layer on the hafnium zirconium oxide film as the second electrode includes: depositing an 80nm third metal layer on the hafnium zirconium oxide film using physical vapor deposition as the second electrode, ie, a metal top electrode.

[0038] Specifically, choose a suitable third metal: the metal used as the second electrode needs to have good conductivity, good contact performance with HZO, and chemical stability in the target application. Commonly used metals include aluminum (Al), titanium (Ti), platinum (Pt), gold (Au), iridium (Ir), etc.

[0039] Combined with Figure 8 , a graph containing three sub-graphs, showing the change of current over time when the device is in use at different voltages.

[0040] The first sub-graph: The voltage is 2.1V. You can see that the current has some spikes on the time axis. These spikes are marked as "Fire", indicating that at this voltage, the system has reached the trigger threshold and has responded. Second sub-graph: The voltage is 2V. Compared with the first sub-graph, the number of current spikes at this voltage is reduced, but there are still multiple spikes marked as "Fire", indicating that at this voltage, the system can also reach the trigger threshold and generate a response; The third sub-graph shows that the voltage is 1.5V. At this lower voltage, the current curve has no obvious spikes, and all the places marked as "Fire failed" indicate that the system failed to reach the trigger threshold and therefore did not respond. As the voltage decreases, the number of times the system reaches the trigger threshold and responds gradually decreases. When the voltage is lower than a certain value (1.5V in this example), the system can no longer reach the trigger threshold and respond. This device is sensitive to voltage and requires a certain voltage to work properly.

[0041] For ease of understanding, this embodiment further illustrates the specific implementation process of the above method in combination with a specific application scenario system.

[0042] Step 1, such as Figure 1 As shown, a substrate 1 is provided, the substrate 1 is cleaned by an RCA cleaning process, and then the substrate 1 is dried by nitrogen gas; Step 2, such as Figure 2 As shown, a first metal layer 2 is generated on a substrate 1 as a first electrode. The first metal layer 2 is deposited by physical vapor deposition, and the thickness of the first metal layer 2 is 80 nm. Step 3, such as Figure 3 As shown, a hafnium zirconium oxide film 3 is formed on the first metal layer 2, and the hafnium zirconium oxide film 3 is deposited by plasma atomic layer deposition. When the reaction temperature is 250° C., the deposition rate is 0.1 nm per cycle. During the deposition process, after each hafnium source gas is introduced for a deposition cycle, the zirconium source gas is continuously introduced for nine deposition cycles. The deposition thickness of the hafnium zirconium oxide film 3 is 6 nm. Step 4, such as Figure 4 As shown, a second metal layer 4 is formed on the hafnium zirconium oxide film 3, and the second metal layer 4 is deposited by physical vapor deposition. The thickness of the second metal layer 4 is 80 nm. After the second metal layer 4 is deposited by physical vapor deposition, the antiferroelectric artificial neuron device is treated at 550° C. for 30 seconds by rapid thermal processing technology; Step 5, such as Figure 5 As shown, the second metal layer 4 is subjected to an etching process, and the second metal layer is etched using a wet etching process, and the composition ratio of the wet etching solution is as follows: ; Step 6, such as Figure 6 As shown, a third metal layer 5 is formed on the hafnium zirconium oxide film 3, and a 80 nm third metal layer is deposited on the hafnium zirconium oxide film using physical vapor deposition to serve as a second electrode, ie, a metal top electrode.

[0043] In some specific embodiments, an antiferroelectric artificial neuron device is also provided, which is manufactured by the method described in the above embodiment and includes a substrate, a first metal layer, a hafnium zirconium oxide film and a third metal layer arranged in sequence.

[0044] In some specific embodiments, the thickness of the first metal layer is 80 nm, the thickness of the hafnium zirconium oxide film is 6 nm, the thickness of the second metal layer is 80 nm, and the thickness of the third metal layer is 80 nm.

[0045] Through the description of the above implementation methods, technicians in the relevant field can clearly understand that for the convenience and simplicity of description, only the division of the above functional modules is used as an example. In actual applications, the above functions can be assigned to different functional modules as needed, that is, the internal structure of the device is divided into different functional modules to complete all or part of the functions described above. The specific working process of the system, device and unit described above can refer to the corresponding process in the aforementioned method embodiment, and will not be repeated here.

[0046] Although the embodiments of the present invention are described in detail above, it is obvious to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations are within the scope and spirit of the present invention as described in the claims. Moreover, the present invention described herein may have other embodiments and may be implemented or realized in a variety of ways.

Claims

1. A method for preparing an antiferroelectric artificial neuron device, characterized in that: include: providing a substrate; forming a first metal layer on the substrate as a first electrode; forming a hafnium zirconium oxide thin film on the first metal layer; forming a second metal layer on the hafnium zirconium oxide film; The hafnium zirconium oxide thin film is crystallized and antiferroelectricity is generated by rapid thermal processing; removing the second metal layer; A third metal layer is formed on the hafnium zirconium oxide film to serve as a second electrode.

2. The method according to claim 1, characterized in that Providing the substrate includes: performing an RCA cleaning process on the substrate, and then drying the substrate with nitrogen.

3. The method according to claim 1, characterized in that Forming a first metal layer on a substrate as a first electrode includes: depositing the first metal layer using a physical vapor deposition method, wherein the first metal layer has a thickness of 80 nm.

4. The method according to claim 1, characterized in that: Forming a hafnium zirconium oxide thin film on the first metal layer includes: The hafnium zirconium oxide film was deposited by plasma atomic layer deposition. When the reaction temperature was 250°C, the deposition rate was 0.1 nm per cycle.

5. The method according to claim 4, characterized in that Deposition of hafnium zirconium oxide thin films using plasma atomic layer deposition, including: During the deposition process, after each hafnium source gas is introduced for a deposition cycle, the zirconium source gas is introduced nine times in succession for deposition cycles. The deposition thickness of the hafnium zirconium oxide film is 6 nm.

6. The method according to claim 1, characterized in that forming a second metal layer on the hafnium zirconium oxide film, comprising: The second metal layer is deposited by physical vapor deposition. The thickness of the second metal layer is 80 nm.

7. The method according to claim 1, characterized in that The antiferroelectric artificial neuron device was treated at 550℃ for 30 seconds by rapid thermal processing technology.

8. The method according to claim 1, characterized in that Removing the second metal layer includes: The two metal layers are etched using a wet etching process, and the composition ratio of the wet etching solution is: NH4H2O∶H2O2∶H2O=1∶2∶5.

9. The method according to claim 1, characterized in that: A third metal layer is formed on the hafnium zirconium oxide film as a second electrode including: An 80 nm third metal layer is deposited on the hafnium zirconium oxide film using physical vapor deposition.

10. An antiferroelectric artificial neuron device, characterized in that: The invention comprises a substrate, a first metal layer, a hafnium zirconium oxide film and a third metal layer which are arranged in sequence.

11. The antiferroelectric artificial neuron device according to claim 10, characterized in that: The substrate is a SiO2 / Si substrate, the first metal layer has a thickness of 80 nm, the hafnium zirconium oxide film has a thickness of 6 nm, the second metal layer has a thickness of 80 nm, and the third metal layer has a thickness of 80 nm.