Forming method of carbon dioxide adsorbent sheet
By superimposing multi-layer carbon dioxide adsorbent tablets, combining ceramic substrates and nano-scale metal aluminum oxide with high content of polyamine groups, the problems of low efficiency and high energy consumption in carbon dioxide adsorbent molding technology are solved, and the problem of low efficiency and high energy consumption in carbon dioxide adsorbent molding technology is achieved. Efficient carbon dioxide capture and desorption improves the processing capacity and environmental protection of the equipment.
Patent Information
- Application Number
- CN202411080522.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The current carbon dioxide adsorbent molding technology has problems such as low efficiency, insufficient processing capacity and long desorption time, resulting in low carbon dioxide capture efficiency and high energy consumption.
Using the design of superimposed multi-layer carbon dioxide adsorbent tablets, the contact area and path of the adsorbent with air is optimized by neatly arranged and closely bonding the spherical particles of carbon dioxide adsorbent in the box, and the contact area and path of the adsorbent with air are combined, and the ceramic substrate and high-content polyamine group are combined. The functionalized nano-scale metal aluminum oxide acts as an adsorbent to form a rich mesoporous structure and surface oxygen-containing functional groups.
It significantly improves the air volume and adsorption efficiency per unit time, shortens adsorption and desorption time, reduces energy consumption, enhances the processing capacity and continuous working capacity of the adsorption tower, and improves the carbon dioxide capture efficiency and the environmental protection of the equipment.
Smart Images

Figure CN118925698A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon dioxide adsorption, and in particular relates to a method for forming a carbon dioxide adsorbent sheet. Background Art
[0002] Since the last century, the process of urbanization and industrialization has accelerated. The large amount of greenhouse gases emitted in this process, especially carbon dioxide, has had a profound impact on the global climate. These emissions have led to a series of serious environmental problems such as global warming. The United Nations Intergovernmental Panel on Climate Change (IPCC) warned in its 2021 report that global warming will reach catastrophic levels in the next two decades. In order to avoid the serious consequences of climate change, many countries around the world have pledged to achieve the goal of net zero CO2 emissions;
[0003] The International Energy Agency (IEA) has made an estimate and pointed out that in order to control the global temperature rise within 1.5℃ by the end of this century, 32% of the carbon emission reduction task needs to be achieved by carbon dioxide capture, utilization and storage (CCUS) technology. This technology is considered one of the key means to mitigate climate change;
[0004] With the continuous development of science and technology, the connotation of CCUS technology is also constantly enriched and improved. In the "Fourth National Assessment Report on Climate Change" released by my country in 2022, negative emission technologies such as biomass carbon capture and storage (BECCS) and direct air capture (DAC) are clearly included in the scope of CCUS technology;
[0005] Compared with other carbon capture technologies, DAC technology has significant advantages. It is not restricted by geographical location and can place the capture point and storage point in the same place, thus greatly reducing transportation costs. At the same time, DAC technology can also effectively solve the emission problems of many CO2 distribution sources such as transportation and construction industries. In addition, since it captures carbon dioxide directly from the air, it can avoid the adsorption / absorbent performance being affected by high concentrations of pollutants in the flue gas (such as NOx, SOx, etc.). These advantages make DAC technology considered to be a highly promising carbon capture technology, which is expected to make important contributions to global carbon emission reduction in the future.
[0006] The biggest challenge currently encountered by the DAC industry is the molding of carbon dioxide adsorbents. To this end, a molding method for carbon dioxide adsorbent sheets has been developed. Summary of the invention
[0007] The object of the present invention is to provide a method for forming a carbon dioxide adsorbent sheet to solve the problems raised in the above background technology.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] A method for forming a carbon dioxide adsorbent sheet comprises the following steps:
[0010] S1, preparation stage: select spherical particles of carbon dioxide adsorbent with a diameter of 3-5mm, ensure that the particles are of uniform quality and have no damage or defects, and prepare a box of appropriate size, which is determined according to the final size and shape of the desired adsorbent sheet;
[0011] S2. Arrangement and glue coating: Arrange the single-layer spherical particles of carbon dioxide adsorbent neatly in the frame. The particles should be in close contact with each other without gaps. Use polymer glue to evenly apply it on the adjacent contact surfaces of each column or row of the adsorbent spherical particles to ensure that the glue layer is thin and uniform.
[0012] S3, tightening and shaping: appropriately tighten the square frame so that the spherical carbon dioxide adsorbent particles are tightly bonded in rows or columns in the square frame. The tightening force should be moderate to avoid damaging the adsorbent particles. During the tightening process, a pit will naturally form between every four adjacent spherical adsorbent particles. These pits will be used for the subsequent laying of the second layer of adsorbent particles.
[0013] S4. Apply glue again: Apply special polymer glue around each pit, making sure that the glue layer covers the edge of the pit and slightly exceeds it, so as to form a good bond with the second layer of adsorbent particles;
[0014] S5. Laying the second layer: Lay a new layer of spherical carbon dioxide adsorbent particles in the pits where the glue is applied, ensuring that these particles are tightly bonded to the first layer of particles. After laying, gently press the second layer of particles to make them in close contact with the first layer of particles and the bottom of the frame to form an adsorbent sheet with two layers of adsorbent particles bonded together.
[0015] S6. Final molding: Take the molded adsorbent sheet out of the frame and perform necessary trimming and inspection to ensure that the quality of the adsorbent sheet meets the requirements.
[0016] Preferably, the adsorbent spherical particles are composed of a ceramic substrate and are coated with a layer of CO2 adsorbent on the outside.
[0017] Preferably, the preparation method of the adsorbent spherical particles is specifically:
[0018] S11, ceramic substrate preparation: by exfoliating the stacked nano-scale metal aluminum oxide precursor, a rich mesoporous structure and surface oxygen-containing functional groups are formed;
[0019] S12, CO2 adsorbent preparation: preparation of nano-scale metal alumina adsorbent functionalized with high content of polyamine groups;
[0020] S13, coating: dispersing the prepared CO2 adsorbent powder in a solvent, adding an appropriate amount of a binder and a dispersant, stirring evenly to form a stable coating liquid, and evenly coating the coating liquid on the surface of the ceramic substrate by an immersion coating method, drying the coated ceramic substrate, removing the solvent, and preliminarily solidifying the coating layer;
[0021] S14, post-processing the coated ceramic substrate.
[0022] Preferably, in S11, a mesoporous structure is formed, the pore size distribution is between 2-50 nm, and the specific surface area is ≥100 m 2 / g, surface oxygen-containing functional group concentration ≥5%.
[0023] Preferably, in S12, the adsorbent powder has a particle size of ≤100 nm and a specific surface area of ≥150 m 2 / g.
[0024] Preferably, in S13, the CO2 adsorbent powder is 50wt%, the solvent is one of deionized water or ethanol, the binder is polyvinyl alcohol, which is 3wt%, the dispersant is carboxymethyl cellulose, which is 1wt%, and the drying treatment is drying at 80°C for 4 hours.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The present invention adopts a design of stacking multiple layers of adsorbent sheets. Compared with the traditional method of directly stacking spherical adsorbent particles in the carbon dioxide adsorption tower, under the same working conditions, the design of the present invention increases the air volume passing through the adsorption tower per unit time by more than 2 times. This improvement not only enhances the processing capacity of the adsorption tower, but also makes the adsorption process more efficient. At the same time, since the design of stacking multiple layers of adsorbent sheets optimizes the contact area and path between the adsorbent and the air, the time for the same weight of adsorbent in the adsorption tower to adsorb carbon dioxide to saturation is greatly shortened to more than half. This means that in the same time, the present invention can adsorb more carbon dioxide, or the time required to reach the saturated adsorption state is shorter, thereby improving the overall work efficiency.
[0027] (2) The stacked multi-layer adsorbent sheet design of the present invention also effectively shortens the desorption time of carbon dioxide, also by more than half. This improvement enables the adsorbent to release the adsorbed carbon dioxide more quickly to prepare for the next round of adsorption process, further improving the continuous working capacity of the adsorption tower. Due to the improved efficiency of the adsorption and desorption processes, the energy consumption of the present invention is also greatly reduced, which not only reduces operating costs, but also makes the technology more environmentally friendly and sustainable in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is a process flow chart of the present invention;
[0029] Figure 2 It is a schematic diagram of the structure of the present invention. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Embodiment 1:
[0032] See also Figure 1 As shown, a method for forming a carbon dioxide adsorbent sheet comprises the following steps:
[0033] S1, preparation stage: select spherical particles of carbon dioxide adsorbent with a diameter of 3-5mm, ensure that the particles are of uniform quality and have no damage or defects, and prepare a box of appropriate size, which is determined according to the final size and shape of the desired adsorbent sheet;
[0034] S2. Arrangement and glue coating: Arrange the single-layer spherical particles of carbon dioxide adsorbent neatly in the frame. The particles should be in close contact with each other without gaps. Use polymer glue to evenly apply it on the adjacent contact surfaces of each column or row of the adsorbent spherical particles to ensure that the glue layer is thin and uniform.
[0035] S3, tightening and shaping: appropriately tighten the square frame so that the spherical carbon dioxide adsorbent particles are tightly bonded in rows or columns in the square frame. The tightening force should be moderate to avoid damaging the adsorbent particles. During the tightening process, a pit will naturally form between every four adjacent spherical adsorbent particles. These pits will be used for the subsequent laying of the second layer of adsorbent particles.
[0036] S4. Apply glue again: Apply special polymer glue around each pit, making sure that the glue layer covers the edge of the pit and slightly exceeds it, so as to form a good bond with the second layer of adsorbent particles;
[0037] S5. Laying the second layer: Lay a new layer of spherical carbon dioxide adsorbent particles in the pits where the glue is applied, ensuring that these particles are tightly bonded to the first layer of particles. After laying, gently press the second layer of particles to make them in close contact with the first layer of particles and the bottom of the frame to form an adsorbent sheet with two layers of adsorbent particles bonded together.
[0038] S6. Final molding: Take the molded adsorbent sheet out of the frame and perform necessary trimming and inspection to ensure that the quality of the adsorbent sheet meets the requirements.
[0039] In one embodiment of the present invention, the spherical adsorbent particles are composed of a ceramic substrate and are coated with a layer of CO2 adsorbent on the outside.
[0040] In one embodiment of the present invention, the method for preparing the adsorbent spherical particles is specifically:
[0041] S11, ceramic substrate preparation: by exfoliating the stacked nano-scale metal aluminum oxide precursor, a rich mesoporous structure and surface oxygen-containing functional groups are formed;
[0042] S12, CO2 adsorbent preparation: preparation of nano-scale metal alumina adsorbent functionalized with high content of polyamine groups;
[0043] S13, coating: dispersing the prepared CO2 adsorbent powder in a solvent, adding an appropriate amount of a binder and a dispersant, stirring evenly to form a stable coating liquid, and evenly coating the coating liquid on the surface of the ceramic substrate by an immersion coating method, drying the coated ceramic substrate, removing the solvent, and preliminarily solidifying the coating layer;
[0044] S14, post-processing the coated ceramic substrate.
[0045] In one embodiment of the present invention, in S11, a mesoporous structure is formed, the pore size distribution is between 2-50 nm, the specific surface area is ≥100 m2 / g, and the concentration of surface oxygen-containing functional groups is ≥5%.
[0046] In one embodiment of the present invention, in S12, the adsorbent powder has a particle size of ≤100 nm and a specific surface area of ≥150 m2 / g.
[0047] In one embodiment of the present invention, in S13, the CO2 adsorbent powder is 50wt%, the solvent is one of deionized water or ethanol, the binder is polyvinyl alcohol, which is 3wt%, the dispersant is carboxymethyl cellulose, which is 1wt%, and the drying treatment is drying at 80°C for 4 hours.
[0048] In the adsorption tower of the DAC device, we first stack the adsorbent sheets with fixed length and width to a suitable height. Since the adsorbent particles are spherical, this design naturally leaves a certain gap between each adsorbent sheet. When the fan in the carbon dioxide adsorption tower is started, it will drive the air to pass smoothly through these gaps. This design not only reduces wind resistance, but also significantly increases the amount of air passing through per unit time. Since the air circulation is smoother, the energy consumption of the equipment during operation is also reduced, thereby improving the overall operating efficiency.
[0049] When the adsorbent sheet needs to be replaced, the operation process is also extremely simple. You only need to carefully take out the old adsorbent sheet from the adsorption tower, and then stack the new adsorbent sheet into the adsorption tower in the same way. This design not only simplifies the steps of replacing the adsorbent sheet, but also ensures that the adsorption tower can operate continuously and efficiently, providing strong support for the capture and treatment of carbon dioxide.
[0050] As can be seen from the above, the mesopores (pore size between 2-50 nanometers) formed during the stripping process can significantly increase the specific surface area of the material. The increase in specific surface area means that more active sites are exposed, thereby improving the adsorption, catalytic and other properties of the material. The rich oxygen-containing functional groups on the surface (such as hydroxyl, carboxyl, etc.) can increase the affinity of the material to gas molecules and improve the adsorption efficiency. These functional groups can serve as adsorption sites to form chemical bonds or hydrogen bonds with gas molecules, thereby effectively capturing gas molecules. Nano-scale metal alumina with high specific surface area and rich mesoporous structure is not only a good adsorbent, but also an excellent catalyst carrier. Its surface oxygen-containing functional groups and mesoporous structure can provide more catalytic active sites, which is conducive to the dispersion and stability of the catalyst, thereby improving the efficiency and selectivity of the catalytic reaction.
[0051] Experimental Example 1:
[0052] 1. Preparation stage:
[0053] In the DAC (direct air capture) device, two adsorption towers are selected, named Tower A and Tower B. Tower A is loaded with 10 kg of multi-layered carbon dioxide adsorbent sheets, while Tower B is loaded with 10 kg of the same type of unformed granular adsorbent. Subsequently, the two adsorption towers are closed and ready for startup operation.
[0054] 2. Desorption process of tower A:
[0055] Start the DAC device and allow Tower A to begin the desorption process, which lasts for 2 hours until the carbon dioxide outlet analyzer of the DAC device shows that the carbon dioxide concentration returns to zero, indicating that the adsorbent in Tower A has been completely desorbed.
[0056] 3. Tower A adsorption process:
[0057] Then, Tower A starts the adsorption process. The fan operating frequency is set to keep the air volume at 1000NM3 / H. The monitoring data of the exhaust carbon dioxide analyzer of the DAC equipment shows that the carbon dioxide concentration in the exhaust gas first decreases from 400ppm to 50ppm, and then gradually increases until it finally shows 400ppm again. At this time, the carbon dioxide adsorbent in Tower A has been saturated with adsorption, and the metered adsorption time is 1 hour.
[0058] 4. Tower A desorption and storage:
[0059] After Tower A is saturated with adsorption, the carbon dioxide storage tank of the DAC device is emptied and evacuated, and Tower A begins the desorption process. The desorbed carbon dioxide is collected in the carbon dioxide storage tank. After 30 minutes of desorption, the carbon dioxide outlet analyzer of the DAC device shows that the carbon dioxide concentration returns to zero, indicating that the desorption of Tower A is completed.
[0060] 5. Tower B operation process:
[0061] According to the operating parameters of tower A, the same operation is performed on tower B. The adsorption air volume is set to 328NM3 / H, the adsorption saturation time is 3 hours, and the desorption time is 2 hours.
[0062] 6. Repeat the experiment and collect data:
[0063] The operation process of tower A and tower B was repeated 5 times each. After collecting data, it was found that the gas pressure in the carbon dioxide storage tank of tower A was 0.2MPa, the rated volume of the gas storage tank was 1 cubic meter, the carbon dioxide purity was 95.4%, and the actual weight of captured carbon dioxide was about 3.4Kg;
[0064] The data of Tower B is similar to that of Tower A: the gas pressure in the CO2 storage tank is 0.2MPa, the rated volume of the gas storage tank is 1 cubic meter, the CO2 purity is 95.2%, and the actual weight of captured CO2 is also about 3.4Kg;
[0065] Experimental Example 2:
[0066] 1. Preparation stage:
[0067] In the DAC (direct air capture) device, two adsorption towers are selected, named Tower A and Tower B. Tower A is loaded with 20 kg of multi-layered carbon dioxide adsorbent sheets, and Tower B is loaded with 20 kg of the same type of unformed granular adsorbent. The two adsorption towers are closed to ensure the airtightness of the system, ready for startup operation.
[0068] 2. Desorption process of tower A:
[0069] Start the DAC device and allow Tower A to begin the desorption process, which lasts for 2 hours and is monitored by the CO2 outlet analyzer of the DAC device until the CO2 concentration display returns to zero, indicating that the adsorbent in Tower A has been completely desorbed.
[0070] 3. Tower A adsorption process:
[0071] Then, the adsorption process starts in Tower A. The operating frequency of the fan is set to keep the air volume at 2000NM3 / H to ensure sufficient air flow through the adsorbent.
[0072] The data monitored by the tail gas carbon dioxide analyzer of the DAC equipment showed that the carbon dioxide concentration in the tail gas first decreased from 400ppm to 50ppm, which was a manifestation of the effective adsorption of carbon dioxide by the adsorbent. As time went on, the carbon dioxide concentration in the tail gas gradually increased until it finally showed 400ppm again. At this time, the carbon dioxide adsorbent in Tower A has been saturated with adsorption, and the metered adsorption time is 1 hour.
[0073] 4. Tower A desorption and storage:
[0074] After Tower A is saturated with adsorption, the carbon dioxide storage tank of the DAC device is emptied and evacuated to prepare for collecting new carbon dioxide. Tower A begins the desorption process, and the desorbed carbon dioxide is collected in the carbon dioxide storage tank. After 30 minutes of desorption, the carbon dioxide outlet analyzer of the DAC device shows that the carbon dioxide concentration returns to zero, indicating that the desorption of Tower A is completed.
[0075] 5. Tower B operation process:
[0076] According to the operating parameters of Tower A, the same operation was performed on Tower B. The adsorption air volume was set to 651NM3 / H to explore the effect of different air volumes on the adsorption effect. The adsorption saturation time was 3 hours and the desorption time was 2 hours, which was consistent with the operating time of Tower A.
[0077] 6. Repeat the experiment and collect data:
[0078] The operation process of the above tower A and tower B was repeated 5 times each to ensure the reliability and stability of the data. After collecting the data, it was found that the gas pressure in the carbon dioxide storage tank of tower A was 0.4MPa, the rated volume of the gas storage tank was 1 cubic meter, the carbon dioxide purity was 95.3%, and the actual weight of captured carbon dioxide was about 6.9Kg.
[0079] The data of Tower B is similar to that of Tower A: the gas pressure in the carbon dioxide storage tank is 0.4MPa, the rated volume of the gas tank is 1 cubic meter, the carbon dioxide purity is 95.3%, and the actual weight of captured carbon dioxide is also about 6.9Kg.
[0080] As can be seen from the above, the present invention has shown significant advantages over the traditional method of directly stacking spherical adsorbent particles in the carbon dioxide adsorption tower by adopting a design of stacking multiple layers of adsorbent sheets. Under the same working conditions, the design of the present invention increases the air volume passing through the adsorption tower per unit time by more than 2 times. This improvement not only enhances the processing capacity of the adsorption tower, but also makes the adsorption process more efficient;
[0081] At the same time, since the design of stacking multiple layers of adsorbent sheets optimizes the contact area and path between the adsorbent and the air, the time for the adsorbent of the same weight in the adsorption tower to adsorb carbon dioxide to saturation is greatly shortened by more than half, which means that in the same time, the present invention can adsorb more carbon dioxide, or the time required to reach the saturated adsorption state is shorter, thereby improving the overall work efficiency;
[0082] In addition, the stacked multi-layer adsorbent sheet design of the present invention also effectively shortens the desorption time of carbon dioxide, also by more than half. This improvement enables the adsorbent to release the adsorbed carbon dioxide faster, preparing for the next round of adsorption process, and further improving the continuous working capacity of the adsorption tower;
[0083] Most importantly, due to the improved efficiency of the adsorption and desorption processes, the energy consumption of the present invention is also greatly reduced, which not only reduces operating costs but also makes the technology more environmentally friendly and sustainable in practical applications.
[0084] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for forming a carbon dioxide adsorbent sheet, characterized in that: The following steps are involved: S1, preparation stage: select spherical particles of carbon dioxide adsorbent with a diameter of 3-5mm, ensure that the particles are of uniform quality and have no damage or defects, and prepare a box of appropriate size, which is determined according to the final size and shape of the desired adsorbent sheet; S2. Arrangement and glue coating: Arrange the single-layer spherical particles of carbon dioxide adsorbent neatly in the frame. The particles should be in close contact with each other without gaps. Use polymer glue to evenly apply it on the adjacent contact surfaces of each column or row of the adsorbent spherical particles to ensure that the glue layer is thin and uniform. S3, tightening and shaping: appropriately tighten the square frame so that the spherical carbon dioxide adsorbent particles are tightly bonded in rows or columns in the square frame. The tightening force should be moderate to avoid damaging the adsorbent particles. During the tightening process, a pit will naturally form between every four adjacent spherical adsorbent particles. These pits will be used for the subsequent laying of the second layer of adsorbent particles. S4. Apply glue again: Apply special polymer glue around each pit, making sure that the glue layer covers the edge of the pit and slightly exceeds it, so as to form a good bond with the second layer of adsorbent particles; S5. Laying the second layer: Lay a new layer of spherical carbon dioxide adsorbent particles in the pits where the glue is applied, ensuring that these particles are tightly bonded to the first layer of particles. After laying, gently press the second layer of particles to make them in close contact with the first layer of particles and the bottom of the frame to form an adsorbent sheet with two layers of adsorbent particles bonded together. S6. Final molding: Take the molded adsorbent sheet out of the frame and perform necessary trimming and inspection to ensure that the quality of the adsorbent sheet meets the requirements.
2. The method for forming a carbon dioxide adsorbent sheet according to claim 1, characterized in that: The adsorbent spherical particles are composed of a ceramic substrate and are coated with a layer of CO2 adsorbent on the outside.
3. The method for forming a carbon dioxide adsorbent sheet according to claim 1, characterized in that: The preparation method of the adsorbent spherical particles is specifically as follows: S11, ceramic substrate preparation: by exfoliating the stacked nano-scale metal aluminum oxide precursor, a rich mesoporous structure and surface oxygen-containing functional groups are formed; S12, CO2 adsorbent preparation: preparation of nano-scale metal alumina adsorbent functionalized with high content of polyamine groups; S13, coating: dispersing the prepared CO2 adsorbent powder in a solvent, adding an appropriate amount of a binder and a dispersant, stirring evenly to form a stable coating liquid, and evenly coating the coating liquid on the surface of the ceramic substrate by an immersion coating method, drying the coated ceramic substrate, removing the solvent, and preliminarily solidifying the coating layer; S14, post-processing the coated ceramic substrate.
4. The method for forming a carbon dioxide adsorbent sheet according to claim 1, characterized in that: In the S11, a mesoporous structure is formed, the pore size distribution is between 2-50nm, and the specific surface area is ≥100m 2 / g, surface oxygen functional group concentration ≥5%.
5. The method for forming a carbon dioxide adsorbent sheet according to claim 1, characterized in that: In S12, the adsorbent powder has a particle size of ≤100 nm and a specific surface area of ≥150 m 2 / g.
6. The method for forming a carbon dioxide adsorbent sheet according to claim 1, characterized in that: In the S13, the CO2 adsorbent powder is 50wt%, the solvent is one of deionized water or ethanol, the binder is polyvinyl alcohol, which is 3wt%, the dispersant is carboxymethyl cellulose, which is 1wt%, and the drying treatment is drying at 80°C for 4 hours.